Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox. Information about Biopolymers, a project by FH Hannover and M-Base Engineering & Software GmbH sponsored by Fachagentur Nachwachsende Rohstoffe (FNR).

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Bayblend® FR3008 RE - (PC+ABS) FR(40) - Covestro Deutschland AG

Material Data Center offers the following functions for Bayblend® FR3008 RE:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Bayblend datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
  • (PC+ABS)-Blend
  • flame retardant
  • Vicat/B 120 temperature = 103 °C
  • improved chemical resistance
  • HDT/A >= 85 °C
  • UL recognition 94 V-0 at 1.5 mm
  • glow wire temperature (GWFI): 960 °C at 2.0 mm
  • good light stability
Partially bio-circular grade / Attributed via mass balance (according to ISCC PLUS Standard).
Processing/Physical CharacteristicsValueUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 13 cm³/10min ISO 1133
Temperature 240 °C -
Load 5 kg -
Molding shrinkage, parallel 0.6 % ISO 294-4, 2577
Molding shrinkage, normal 0.6 % ISO 294-4, 2577
Mechanical propertiesValueUnitTest Standard
ISO Data
Tensile Modulus 2800 MPa ISO 527
Yield stress 60 MPa ISO 527
Yield strain 4 % ISO 527
Flexural modulus, 23°C 2700 MPa ISO 178
Flexural strength 98 MPa ISO 178
Izod impact strength, +23°C N kJ/m² ISO 180/1U
Izod notched impact strength, +23°C 30 kJ/m² ISO 180/1A
Izod notched impact strength 10 kJ/m² ISO 180/1A
Temperature -30 °C -
Thermal propertiesValueUnitTest Standard
ISO Data
Temp. of deflection under load, 1.80 MPa 85 °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 95 °C ISO 75-1/-2
Vicat softening temperature, B 101 °C ISO 306
Coeff. of linear therm. expansion, parallel 76 E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion, normal 80 E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. V-0 class IEC 60695-11-10
Thickness tested 1.5 mm -
Yellow Card available yes - -
Burning Behav. 5V at thickness h 5VB class IEC 60695-11-20
Thickness tested 2.0 mm -
Yellow Card available yes - -
Oxygen index 32 % ISO 4589-1/-2
Glow Wire Flammability Index (GWFI) 960 °C IEC 60695-2-12
GWFI - thickness tested (1) 2 mm -
Electrical propertiesValueUnitTest Standard
ISO Data
Relative permittivity, 100Hz 3.2 - IEC 62631-2-1
Relative permittivity, 1MHz 3.1 - IEC 62631-2-1
Dissipation factor, 100Hz 50 E-4 IEC 62631-2-1
Dissipation factor, 1MHz 70 E-4 IEC 62631-2-1
Volume resistivity >1E13 Ohm*m IEC 62631-3-1
Surface resistivity >1E15 Ohm IEC 62631-3-2
Electric strength 30 kV/mm IEC 60243-1
Comparative tracking index 300 - IEC 60112
Other propertiesValueUnitTest Standard
Water absorption 0.5 % Sim. to ISO 62
Humidity absorption 0.2 % Sim. to ISO 62
Density 1180 kg/m³ ISO 1183
Test specimen productionValueUnitTest Standard
ISO Data
Injection Molding, melt temperature 240 °C ISO 294
Injection Molding, mold temperature 80 °C ISO 294
Injection Molding, injection velocity 240 mm/s ISO 294
Processing Recommendation Injection MoldingValueUnitTest Standard
Pre-drying - Temperature 80 °C -
Pre-drying - Time 4 h -
Processing humidity ≤0.02 % -
Melt temperature 240 - 270 °C -
Mold temperature 60 - 90 °C -
Zone 1 220 - 230 °C -
Zone 2 225 - 235 °C -
Zone 3 230 - 240 °C -
Nozzle temperature 255 - 265 °C -
Back pressure 5 - 15 MPa -
Characteristics
Processing
Injection Molding
Special Characteristics
Flame retardant
Chemical Resistance
General Chemical Resistance
Certifications
Contains renewable resources, ISCC Plus
Regional Availability
North America, Europe, Asia Pacific, South and Central America, Near East/Africa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com