Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of CELSTRAN® PP-GF20-0553 Black - PP-GLF20 - Celanese

Material Data Center offers the following functions for CELSTRAN® PP-GF20-0553 Black:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Celstran datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
Material code according to ISO 1043-1: PP Polypropylene copolymer reinforced with 20weight percent long glass fibers.Black.  Low emission. The fibers are chemically coupled to the polypropylene matrix. The pellets are cylindrical and normally as well as the embedded fibers 11 mm long. Parts molded of CELSTRAN have outstanding mechanical properties such as high strength and stiffness combined with high heat deflection. The notched impact strength is increased at elevated and low temperatures due to the fiber skeleton built in the parts. The long fiber reinforcement reduces creep significantly. The very isotropic shrinkage in the molded parts minimizes the warpage. Complex parts can be manufactured with high reproducibility by injection molding. Application field: Functional/structural parts for automotive

Flammability at thickness h (1 mm)HB-
Processing/Physical CharacteristicsValueUnitTest Standard
ISO Data
Molding shrinkage, parallel 0.4 % ISO 294-4, 2577
Molding shrinkage, normal 0.5 % ISO 294-4, 2577
Mechanical propertiesValueUnitTest Standard
ISO Data
Tensile Modulus 4700 MPa ISO 527
Stress at break 84 MPa ISO 527
Strain at break 2.5 % ISO 527
Charpy impact strength, +23°C 56 kJ/m² ISO 179/1eU
Charpy impact strength, -30°C 60 kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 20 kJ/m² ISO 179/1eA
Charpy notched impact strength, -30°C 20 kJ/m² ISO 179/1eA
Thermal propertiesValueUnitTest Standard
ISO Data
Temp. of deflection under load, 1.80 MPa 159 °C ISO 75-1/-2
Temp. of deflection under load, 8.00 MPa 136 °C ISO 75-1/-2
Burning Behav. at thickness h HB class IEC 60695-11-10
Thickness tested 1.0 mm -
Other propertiesValueUnitTest Standard
Density 1030 kg/m³ ISO 1183
Diagrams
Stress-strain , CELSTRAN® PP-GF20-0553 Black, PP-GLF20, Celanese
Secant modulus-strain , CELSTRAN® PP-GF20-0553 Black, PP-GLF20, Celanese
Stress-strain (isochronous) 23°C, CELSTRAN® PP-GF20-0553 Black, PP-GLF20, Celanese
Creep modulus-time 23°C, CELSTRAN® PP-GF20-0553 Black, PP-GLF20, Celanese
Creep curve 23°C, CELSTRAN® PP-GF20-0553 Black, PP-GLF20, Celanese
Characteristics
Processing
Injection Molding
Delivery form
Pellets, Black
Special Characteristics
Heat stabilized or stable to heat
Features
Chemically Coupled Reinforcement, Creep Resistance, Long fiber reinforced, Low Emission, Low Warpage, Copolymer
Applications
Automotive
Regional Availability
North America, Europe, Asia Pacific
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com