Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Elix ABS M545TF - ABS - Elix Polymers, S.L.

Material Data Center offers the following functions for Elix ABS M545TF:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Elix datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Processing/Physical CharacteristicsValueUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 32 cm³/10min ISO 1133
Temperature 220 °C -
Load 10 kg -
Molding shrinkage, parallel 0.6 % ISO 294-4, 2577
Molding shrinkage, normal 0.6 % ISO 294-4, 2577
Mechanical propertiesValueUnitTest Standard
ISO Data
Tensile Modulus 2250 MPa ISO 527
Yield stress 42 MPa ISO 527
Yield strain 2.6 % ISO 527
Strain at break 25 % ISO 527
Flexural modulus, 23°C 2300 MPa ISO 178
Flexural strength 70 MPa ISO 178
Charpy impact strength, +23°C 110 kJ/m² ISO 179/1eU
Charpy impact strength, -30°C 90 kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 15 kJ/m² ISO 179/1eA
Charpy notched impact strength, -30°C 7 kJ/m² ISO 179/1eA
Izod notched impact strength, +23°C 17 kJ/m² ISO 180/1A
Izod notched impact strength 7 kJ/m² ISO 180/1A
Temperature -30 °C -
Ball indentation hardness 110 MPa ISO 2039-1
Thermal propertiesValueUnitTest Standard
ISO Data
Temp. of deflection under load, 1.80 MPa 94 °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 98 °C ISO 75-1/-2
Vicat softening temperature, B 98 °C ISO 306
Coeff. of linear therm. expansion, parallel 90 E-6/K ISO 11359-1/-2
Glow Wire Flammability Index (GWFI) 700 °C IEC 60695-2-12
GWFI - thickness tested (1) 2 mm -
Electrical propertiesValueUnitTest Standard
ISO Data
Relative permittivity, 100Hz 3 - IEC 62631-2-1
Relative permittivity, 1MHz 2.9 - IEC 62631-2-1
Dissipation factor, 100Hz 50 E-4 IEC 62631-2-1
Dissipation factor, 1MHz 90 E-4 IEC 62631-2-1
Volume resistivity 1E13 Ohm*m IEC 62631-3-1
Surface resistivity 1E15 Ohm IEC 62631-3-2
Electric strength 35 kV/mm IEC 60243-1
Comparative tracking index 600 - IEC 60112
Other propertiesValueUnitTest Standard
Density 1050 kg/m³ ISO 1183
Processing Recommendation Injection MoldingValueUnitTest Standard
Melt temperature 240 °C -
Mold temperature 70 °C -
Injection speed 240 mm/s -
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Certifications
Food contact, RoHS compliant
Regional Availability
Europe, Asia Pacific, South and Central America, Near East/Africa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.