Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Grivory HT1V-5 FWA natural - PA6T/6I-GF50 - EMS-GRIVORY | a unit of EMS-CHEMIE AG

Material Data Center offers the following functions for Grivory HT1V-5 FWA natural:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Grivory datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
Product nomenclature: ISO 16396-PA6T/6I,GF50,M1H,C12-190

 

Co Polyamide

Partially aromatic Polyamide

Product Attributes

  Hydrolysis resistant, Improved heat resistance

Markets

  Industry & Consumer goods
  Housewares, Medical devices, Sanitary, water and gas supply

Approvals

  Food Contact
  NSF 51, EU Requirements, FDA
  Potable Water Contact
  NSF 61, KTW, WRAS, ACS, DVGW W270
Processing/Physical Characteristicsdry / condUnitTest Standard
ISO Data
Molding shrinkage, parallel 0.1 / * % ISO 294-4, 2577
Molding shrinkage, normal 0.5 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
ISO Data
Tensile Modulus 18000 / 17500 MPa ISO 527
Stress at break 250 / 240 MPa ISO 527
Strain at break 2 / 2 % ISO 527
Charpy impact strength, +23°C 80 / 80 kJ/m² ISO 179/1eU
Charpy impact strength, -30°C 80 / 80 kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 11 / 11 kJ/m² ISO 179/1eA
Charpy notched impact strength, -30°C 10 / 10 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
ISO Data
Melting temperature, 10°C/min 325 / * °C ISO 11357-1/-3
Temp. of deflection under load, 8.00 MPa 200 / * °C ISO 75-1/-2
Coeff. of linear therm. expansion, parallel 15 / * E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion, normal 40 / * E-6/K ISO 11359-1/-2
Burning Behav. at thickness h HB / * class IEC 60695-11-10
Thickness tested 0.8 / * mm -
Electrical propertiesdry / condUnitTest Standard
ISO Data
Volume resistivity 1E11 / 1E11 Ohm*m IEC 62631-3-1
Surface resistivity * / 1E12 Ohm IEC 62631-3-2
Electric strength 35 / 35 kV/mm IEC 60243-1
Comparative tracking index - / 600 - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 3 / * % Sim. to ISO 62
Humidity absorption 1.3 / * % Sim. to ISO 62
Density 1650 / - kg/m³ ISO 1183
Characteristics
Processing
Injection Molding
Delivery form
Granules, Natural Color
Special Characteristics
Heat stabilized or stable to heat
Features
Copolymer
Chemical Resistance
Hydrolytically Stable
Certifications
Food contact, Food approval FDA 21 CFR, Food approval NSF 51, Drinking water contact, Drinking water contact KTW, Drinking water contact DVGW W270, Drinking water contact NSF 61
Applications
Medical
Regional Availability
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.