Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of KEPAMID® 2340GM3 - PA66-(GF+MX)40 - Korea Engineering Plastics Co. Ltd.

Material Data Center offers the following functions for KEPAMID® 2340GM3:
unit conversion, PDF datasheet print, comparison with other plastics

Check here, which other Kepamid datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Processing/Physical CharacteristicsValueUnitTest Standard
ISO Data
Molding shrinkage, parallel 0.8 % ISO 294-4, 2577
Mechanical propertiesValueUnitTest Standard
ISO Data
Tensile Strength 118 MPa ISO 527
Strain at break 4 % ISO 527
Flexural modulus, 23°C 6860 MPa ISO 178
Charpy notched impact strength, +23°C 3.5 kJ/m² ISO 179/1eA
Rockwell hardness R121 - ISO 2039-2
Thermal propertiesValueUnitTest Standard
ISO Data
Melting temperature, 10°C/min 260 °C ISO 11357-1/-3
Temp. of deflection under load, 1.80 MPa 235 °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 255 °C ISO 75-1/-2
Burning behav. at thickness h HB class IEC 60695-11-10
Thickness tested 0.8 mm -
Electrical propertiesValueUnitTest Standard
ISO Data
Relative permittivity, 1MHz 3.5 - IEC 62631-2-1
Other propertiesValueUnitTest Standard
Humidity absorption 0.6 % Sim. to ISO 62
Density 1440 kg/m³ ISO 1183
Processing Recommendation Injection MoldingValueUnitTest Standard
Pre-drying - Temperature 80 - 90 °C -
Pre-drying - Time 4 - 8 h -
Processing humidity ≤0.05 % -
Mold temperature 70 - 90 °C -
Feed temperature 60 - 80 °C -
Zone 1 280 °C -
Zone 2 285 °C -
Zone 3 285 °C -
Nozzle temperature 290 °C -
Screw speed 80 - 120 rpm -
Back pressure 0.5 - 1 MPa -
Characteristics
Processing
Injection Molding
Special Characteristics
Heat stabilized or stable to heat
Features
Low Warpage
Applications
Automotive, Electrical and Electronical
Regional Availability
North America, Europe, Asia Pacific
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.