Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of LUMICENE® mPE M 1811 PCE - (PE-LLD+PPA) - TotalEnergies

Material Data Center offers the following functions for LUMICENE® mPE M 1811 PCE:
unit conversion, PDF datasheet print, comparison with other plastics

Check here, which other Lumicene datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
For more detailed information, please read our brochure p. 46 to 54
or contact our representatives in your region.
Processing/Physical CharacteristicsValueUnitTest Standard
ISO Data
Melt flow index, MFI 1 g/10min ISO 1133
Temperature 190 °C -
Load 2.16 kg -
Thermal propertiesValueUnitTest Standard
ISO Data
Melting temperature, 10°C/min 111 °C ISO 11357-1/-3
Optical propertiesValueUnitTest Standard
ISO Data
Haze 4.5 - ISO 14782
ASTM Data
Gloss 76 - ASTM D 2457
Other propertiesValueUnitTest Standard
Density 918 kg/m³ ISO 1183
Film PropertiesValueUnitTest Standard
ISO Data
Stress at yield, parallel 10 MPa ISO 527-3
Stress at yield, normal 10 MPa ISO 527-3
Stress at break, parallel 68 MPa ISO 527-3
Stress at break, normal 62 MPa ISO 527-3
Maximum strain, parallel 670 % ISO 527-3
Maximum strain, normal 700 % ISO 527-3
Dart drop A 1200 g ISO 7765-1
Type of extrusion blown - -
Thickness of specimen 0.04 mm -
Processing Recommendation ExtrusionValueUnitTest Standard
Type of extrusion blown - -
Melt temperature 180 - 230 °C -
Characteristics
Processing
Blown Film Extrusion, Film Extrusion
Additives
Antiblocking agent
Special Characteristics
High impact or impact modified
Features
Blending Resin, Heat Sealable
Chemical Resistance
Oxidation Resistance
Certifications
Food contact
Applications
Packaging
Regional Availability
Europe
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.