Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Luran® S ECO 778T BC30 - ASA - INEOS Styrolution

Material Data Center offers the following functions for Luran® S ECO 778T BC30:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, cooling time calculation, CAE Interfaces

Check here, which other Luran datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
Luran® S ECO 778T BC30 acrylonitrile styrene acrylate (ASA) polymer features high surface quality and good impact strength including enhanced colour fastness. The product delivers superior long-term performance when exposed to UV irradiation and additionally provide excellent chemical resistance. Luran® S ECO 778T BC30 is an injection molding grade with enhanced heat resistance and best chemical resistance among the Luran® S grades. Luran® S ECO 778T BC30 is an ISCC compliant product leading to a substitution of fossil source styrene with ISCC certified bio-attributed styrene.
Carbon Footprint Reduction vs Fossil-Based (3rd party validated): 39 % (ISO 14044)
Attributed Content of ISCC-certified Bio-Circular Sources (min.): 30 %
Processing/Physical CharacteristicsValueUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 5 cm³/10min ISO 1133
Temperature 220 °C -
Load 10 kg -
Molding shrinkage, parallel 0.6 % ISO 294-4, 2577
Density of melt 960 kg/m³ -
Thermal conductivity of melt 0.185 W/(m K) -
Spec. heat capacity of melt 2160 J/(kg K) -
Ejection temperature 98 °C -
Mechanical propertiesValueUnitTest Standard
ISO Data
Tensile Modulus 2500 MPa ISO 527
Yield stress 54 MPa ISO 527
Yield strain 3.4 % ISO 527
Nominal strain at break 8 % ISO 527
Flexural modulus, 23°C 2450 MPa ISO 178
Flexural strength 80 MPa ISO 178
Charpy impact strength, +23°C 220 kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 15 kJ/m² ISO 179/1eA
Charpy notched impact strength, -30°C 4 kJ/m² ISO 179/1eA
Ball indentation hardness 85 MPa ISO 2039-1
Thermal propertiesValueUnitTest Standard
ISO Data
Temp. of deflection under load, 1.80 MPa 103 °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 106 °C ISO 75-1/-2
Vicat softening temperature, B 104 °C ISO 306
Coeff. of linear therm. expansion, parallel 95 E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB class IEC 60695-11-10
Thickness tested 1.5 mm -
Yellow Card available yes - -
Burning Behav. at thickness h HB class IEC 60695-11-10
Thickness tested 3.0 mm -
Yellow Card available yes - -
Burning rate, FMVSS, Thickness 1 mm 30[1] mm/min ISO 3795 (FMVSS 302)
Other Standards[S]
Thermal Conductivity, solid state 0.17 W/(m K) DIN 52612-1
1: 2 mm  S: These properties are reported by the producer according standards that are different to our defaults.
Other propertiesValueUnitTest Standard
Water absorption 1.65 % Sim. to ISO 62
Humidity absorption 0.35 % Sim. to ISO 62
Density 1070 kg/m³ ISO 1183
Bulk density 600 kg/m³ -
Processing Recommendation Injection MoldingValueUnitTest Standard
Pre-drying - Temperature 80 °C -
Pre-drying - Time 2 - 4 h -
Melt temperature 240 - 280 °C -
Mold temperature 40 - 80 °C -
Diagrams
Viscosity-shear rate , Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Shearstress-shear rate , Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Dynamic Shear modulus-temperature , Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Stress-strain , Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Secant modulus-strain , Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Stress-strain (isochronous) 23°C, Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Creep modulus-time 23°C, Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Creep curve 23°C, Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Stress-strain (isochronous) 60°C, Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Creep modulus-time 60°C, Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Creep curve 60°C, Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Specific volume-temperature (pvT) , Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Tensile modulus-temperature , Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Additives
Release agent
Special Characteristics
High impact or impact modified, Light stabilized or stable to light, U.V. stabilized or stable to weather, Heat stabilized or stable to heat
Chemical Resistance
General Chemical Resistance
Certifications
Contains renewable resources, ISCC Plus
Applications
Automotive, Electrical and Electronical, Sports Equipment, Toys
Regional Availability
North America, Europe, Asia Pacific, South and Central America, Near East/Africa
Other text information
Injection molding
PREPROCESSING

Pre-drying, Temperature: 80°C

Pre-drying, Time: 2 - 4h

PROCESSING

Melt temperature, range: 240 - 280°C

Mold temperature, range: 40 - 80°C

Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com