Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Pebax® 5533 SA 01 MED - TPA - ARKEMA

Material Data Center offers the following functions for Pebax® 5533 SA 01 MED:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Pebax datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
Polyether block amide Pebax® 5533 SA 01 MED resin is a thermoplastic elastomer made of flexible polyether and rigid polyamide.
This grade offers the highest quality and it is specially designed to meet the stringent requirements of the medical applications such as minimally invasive devices.
Pebax® 5533 SA 01 MED resin also offers an excellent combination of properties such as: kink resistance, low friction coefficient and superior dynamic response.
Upon request, letters regarding USP Class VI compliance can be provided.


Main applications:
  • Tubings like angiography and angioplasty catheters
  • Flexible injected parts


Packaging:

This grade is delivered dried in sealed packaging (20 kg bags) ready to be processed.

Shelf Life:
Two years from the delivery. For any use above this limit, please refer to our technical services.
Mechanical propertiesdry / condUnitTest Standard
ISO Data
Tensile Modulus 170 / 161 MPa ISO 527
Yield stress 12 / 12 MPa ISO 527
Yield strain 25 / 25 % ISO 527
Nominal strain at break >50 / >50 % ISO 527
Shore D hardness 50 / * - ISO 7619-1
Thermal propertiesdry / condUnitTest Standard
ISO Data
Melting temperature, 10°C/min 159 / * °C ISO 11357-1/-3
Vicat softening temperature, B 66 / * °C ISO 306
Other propertiesdry / condUnitTest Standard
Water absorption 1.2 / * % Sim. to ISO 62
Humidity absorption 0.6 / * % Sim. to ISO 62
Density 1010 / 1010 kg/m³ ISO 1183
Processing Recommendation Injection MoldingValueUnitTest Standard
Pre-drying - Temperature 65 - 75 °C -
Pre-drying - Time 4 - 6 h -
Melt temperature 200 - 270 °C -
Mold temperature 25 - 60 °C -
Characteristics
Processing
Injection Molding, Other Extrusion
Delivery form
Pellets
Special Characteristics
Light stabilized or stable to light, Heat stabilized or stable to heat
Certifications
Medical Grade, US Pharmacopeia Class VI Approved
Regional Availability
Other text information
Injection molding

Processing conditions:

- Typical melt temperature (Min / Recommended / Max) : 200°C / 240°C / 270°C.
- Typical mold temperature : 25 – 60°C.
- Drying time and temperature (only necessary for bags opened for more than two hours) : 4-6 hours at 65-75°C.
Other extrusion

Processing conditions:

- Typical melt temperature (Min / Recommended / Max) : 210°C / 220°C / 230°C.
- Drying time and temperature (only necessary for bags opened for more than two hours) : 4-6 hours at 65-75°C.
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.