Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultradur® B 4300 K6 - PBT-GB30 - BASF

Material Data Center offers the following functions for Ultradur® B 4300 K6:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultradur datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
Injection molding grade with 30 % glass beads and low warpage tendency. To produce technical parts, e.g. in the automotive or electrical industry.The products with the color designations BK15075 and LS BK15091 are optimized for automotive interior applications

Abbreviated designation according to ISO 1043: PBT-GB30
Processing/Physical CharacteristicsValueUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 9 cm³/10min ISO 1133
Temperature 250 °C -
Load 2.16 kg -
Molding shrinkage, parallel 1.7 % ISO 294-4, 2577
Molding shrinkage, normal 1.7 % ISO 294-4, 2577
Mechanical propertiesValueUnitTest Standard
ISO Data
Tensile Modulus 4000 MPa ISO 527
Stress at break 50 MPa ISO 527
Strain at break 5 % ISO 527
Tensile creep modulus, 1000h 2200 MPa ISO 899-1
Charpy impact strength, +23°C 35 kJ/m² ISO 179/1eU
Charpy impact strength, -30°C 24 kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 3 kJ/m² ISO 179/1eA
Thermal propertiesValueUnitTest Standard
ISO Data
Melting temperature, 10°C/min 223 °C ISO 11357-1/-3
Temp. of deflection under load, 1.80 MPa 75 °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 175 °C ISO 75-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB class IEC 60695-11-10
Thickness tested 1.5 mm -
Yellow Card available yes - -
Burning Behav. at thickness h HB class IEC 60695-11-10
Thickness tested 0.8 mm -
Yellow Card available yes - -
Oxygen index 23 % ISO 4589-1/-2
Electrical propertiesValueUnitTest Standard
ISO Data
Relative permittivity, 100Hz 3.8 - IEC 62631-2-1
Relative permittivity, 1MHz 3.8 - IEC 62631-2-1
Dissipation factor, 100Hz 12 E-4 IEC 62631-2-1
Dissipation factor, 1MHz 190 E-4 IEC 62631-2-1
Volume resistivity >1E13 Ohm*m IEC 62631-3-1
Surface resistivity 1E13 Ohm IEC 62631-3-2
Electric strength 37 kV/mm IEC 60243-1
Comparative tracking index 225 - IEC 60112
Other propertiesValueUnitTest Standard
Water absorption 0.4 % Sim. to ISO 62
Humidity absorption 0.2 % Sim. to ISO 62
Density 1530 kg/m³ ISO 1183
Material specific propertiesValueUnitTest Standard
ISO Data
Viscosity number 113 cm³/g ISO 307, 1157, 1628
Test specimen productionValueUnitTest Standard
ISO Data
Injection Molding, melt temperature 250 °C ISO 294
Injection Molding, mold temperature 60 °C ISO 294
Injection Molding, injection velocity 200 mm/s ISO 294
Processing Recommendation Injection MoldingValueUnitTest Standard
Pre-drying - Temperature 80 - 120 °C -
Pre-drying - Time 4 h -
Processing humidity ≤0.04 % -
Melt temperature 250 - 275 °C -
Mold temperature 40 - 80 °C -
Diagrams
Viscosity-shear rate , Ultradur® B 4300 K6, PBT-GB30, BASF
Shearstress-shear rate , Ultradur® B 4300 K6, PBT-GB30, BASF
Stress-strain , Ultradur® B 4300 K6, PBT-GB30, BASF
Secant modulus-strain , Ultradur® B 4300 K6, PBT-GB30, BASF
Stress-strain (isochronous) 23°C, Ultradur® B 4300 K6, PBT-GB30, BASF
Creep modulus-time 23°C, Ultradur® B 4300 K6, PBT-GB30, BASF
Creep curve 23°C, Ultradur® B 4300 K6, PBT-GB30, BASF
Stress-strain (isochronous) 40°C, Ultradur® B 4300 K6, PBT-GB30, BASF
Creep modulus-time 40°C, Ultradur® B 4300 K6, PBT-GB30, BASF
Creep curve 40°C, Ultradur® B 4300 K6, PBT-GB30, BASF
Stress-strain (isochronous) 60°C, Ultradur® B 4300 K6, PBT-GB30, BASF
Creep modulus-time 60°C, Ultradur® B 4300 K6, PBT-GB30, BASF
Creep curve 60°C, Ultradur® B 4300 K6, PBT-GB30, BASF
Stress-strain (isochronous) 90°C, Ultradur® B 4300 K6, PBT-GB30, BASF
Creep modulus-time 90°C, Ultradur® B 4300 K6, PBT-GB30, BASF
Creep curve 90°C, Ultradur® B 4300 K6, PBT-GB30, BASF
Stress-strain (isochronous) 120°C, Ultradur® B 4300 K6, PBT-GB30, BASF
Creep modulus-time 120°C, Ultradur® B 4300 K6, PBT-GB30, BASF
Creep curve 120°C, Ultradur® B 4300 K6, PBT-GB30, BASF
Stress-strain (isochronous) 160°C, Ultradur® B 4300 K6, PBT-GB30, BASF
Creep modulus-time 160°C, Ultradur® B 4300 K6, PBT-GB30, BASF
Creep curve 160°C, Ultradur® B 4300 K6, PBT-GB30, BASF
Tensile modulus-temperature , Ultradur® B 4300 K6, PBT-GB30, BASF
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Additives
Lubricants
Special Characteristics
Light stabilized or stable to light, U.V. stabilized or stable to weather, Heat stabilized or stable to heat
Regional Availability
Other text information
Injection molding
PREPROCESSING
Pre/Post-processing, max. allowed water content: .04 %
Pre/Post-processing, Pre-drying, Temperature: 80 - 120 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 250 - 275 °C
injection molding, Melt temperature, recommended: 250 °C
injection molding, Mold temperature, range: 40 - 80 °C
injection molding, Mold temperature, recommended: 60 °C
Chemical Media Resistance
Acids
Acetic Acid (5% by mass) (23°C)
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com