Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultradur® B 4300 G6 - PBT-GF30 - BASF

Material Data Center offers the following functions for Ultradur® B 4300 G6:
unit conversion, PDF datasheet print, comparison with other plastics, application examples, flow length calculation, snap fit calculation, beam deflection calculation, cooling time calculation, parameters for material models, CAE Interfaces

Check here, which other Ultradur datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
Injection molding grade with 30 % glass fibers. To produce technical parts, e.g. in the automotive or electrical industry. The product with the color designation LS BK15141 is optimized for automotive interior
applications.
The products can also be offered as BMBcert™ and/or Ccycled™. Due to the Massbalance approach the product properties do not change.

Abbreviated designation according to ISO 1043: PBT-GF30
Processing/Physical CharacteristicsValueUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 11 cm³/10min ISO 1133
Temperature 250 °C -
Load 2.16 kg -
Molding shrinkage, parallel 0.3 % ISO 294-4, 2577
Molding shrinkage, normal 1.1 % ISO 294-4, 2577
Density of melt 1300 kg/m³ -
Thermal conductivity of melt 0.22 W/(m K) -
Spec. heat capacity of melt 1770 J/(kg K) -
Ejection temperature 180 °C -
ASTM Data
Mold Shrinkage, MD 0.003 mm/mm ASTM D 955
Mechanical propertiesValueUnitTest Standard
ISO Data
Tensile Modulus 9800 MPa ISO 527
Stress at break 140 MPa ISO 527
Strain at break 3 % ISO 527
Tensile creep modulus, 1000h 7500 MPa ISO 899-1
Charpy impact strength, +23°C 74 kJ/m² ISO 179/1eU
Charpy impact strength, -30°C 74 kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 9 kJ/m² ISO 179/1eA
Charpy notched impact strength, -30°C 8.5 kJ/m² ISO 179/1eA
ASTM Data
Tensile Modulus 9653 MPa ASTM D 638
Tensile Strength at Break 135 MPa ASTM D 638
Elongation at Break 2.5 % ASTM D 638
Flexural Modulus 8067 MPa ASTM D 790
Thermal propertiesValueUnitTest Standard
ISO Data
Melting temperature, 10°C/min 223 °C ISO 11357-1/-3
Temp. of deflection under load, 1.80 MPa 205 °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 220 °C ISO 75-1/-2
Coeff. of linear therm. expansion, parallel 25 E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion, normal 115 E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB class IEC 60695-11-10
Thickness tested 1.5 mm -
Yellow Card available yes - -
Burning Behav. at thickness h HB class IEC 60695-11-10
Thickness tested 0.8 mm -
Yellow Card available yes - -
Oxygen index 19.5 % ISO 4589-1/-2
ASTM Data
DTUL @ 66 psi 220 °C ASTM D 648
DTUL @ 264 psi 210 °C ASTM D 648
Melting Temperature 223 °C ASTM D 3418
Electrical propertiesValueUnitTest Standard
ISO Data
Relative permittivity, 100Hz 4 - IEC 62631-2-1
Relative permittivity, 1MHz 3.8 - IEC 62631-2-1
Dissipation factor, 100Hz 25 E-4 IEC 62631-2-1
Dissipation factor, 1MHz 170 E-4 IEC 62631-2-1
Surface resistivity 1E13 Ohm IEC 62631-3-2
Electric strength 37 kV/mm IEC 60243-1
Comparative tracking index 375 - IEC 60112
Other propertiesValueUnitTest Standard
Water absorption 0.4 % Sim. to ISO 62
Humidity absorption 0.2 % Sim. to ISO 62
Density 1530 kg/m³ ISO 1183
Density 1530 kg/m³ ASTM D 792
Material specific propertiesValueUnitTest Standard
ISO Data
Viscosity number 105 cm³/g ISO 307, 1157, 1628
Test specimen productionValueUnitTest Standard
ISO Data
Injection Molding, melt temperature 260 °C ISO 294
Injection Molding, mold temperature 80 °C ISO 294
Injection Molding, injection velocity 200 mm/s ISO 294
Processing Recommendation Injection MoldingValueUnitTest Standard
Pre-drying - Temperature 80 - 120 °C -
Pre-drying - Time 4 h -
Processing humidity ≤0.04 % -
Melt temperature 250 - 275 °C -
Mold temperature 60 - 100 °C -
Diagrams
Viscosity-shear rate , Ultradur® B 4300 G6, PBT-GF30, BASF
Shearstress-shear rate , Ultradur® B 4300 G6, PBT-GF30, BASF
Dynamic Shear modulus-temperature , Ultradur® B 4300 G6, PBT-GF30, BASF
Stress-strain , Ultradur® B 4300 G6, PBT-GF30, BASF
Secant modulus-strain , Ultradur® B 4300 G6, PBT-GF30, BASF
Stress-strain (isochronous) 23°C, Ultradur® B 4300 G6, PBT-GF30, BASF
Creep modulus-time 23°C, Ultradur® B 4300 G6, PBT-GF30, BASF
Creep curve 23°C, Ultradur® B 4300 G6, PBT-GF30, BASF
Stress-strain (isochronous) 40°C, Ultradur® B 4300 G6, PBT-GF30, BASF
Creep modulus-time 40°C, Ultradur® B 4300 G6, PBT-GF30, BASF
Creep curve 40°C, Ultradur® B 4300 G6, PBT-GF30, BASF
Stress-strain (isochronous) 90°C, Ultradur® B 4300 G6, PBT-GF30, BASF
Creep modulus-time 90°C, Ultradur® B 4300 G6, PBT-GF30, BASF
Creep curve 90°C, Ultradur® B 4300 G6, PBT-GF30, BASF
Stress-strain (isochronous) 120°C, Ultradur® B 4300 G6, PBT-GF30, BASF
Creep modulus-time 120°C, Ultradur® B 4300 G6, PBT-GF30, BASF
Creep curve 120°C, Ultradur® B 4300 G6, PBT-GF30, BASF
Stress-strain (isochronous) 160°C, Ultradur® B 4300 G6, PBT-GF30, BASF
Creep modulus-time 160°C, Ultradur® B 4300 G6, PBT-GF30, BASF
Creep curve 160°C, Ultradur® B 4300 G6, PBT-GF30, BASF
Specific volume-temperature (pvT) , Ultradur® B 4300 G6, PBT-GF30, BASF
Tensile modulus-temperature , Ultradur® B 4300 G6, PBT-GF30, BASF
Characteristics
Processing
Injection Molding
Delivery form
Pellets, Natural Color
Additives
Lubricants
Special Characteristics
Light stabilized or stable to light, U.V. stabilized or stable to weather, Heat stabilized or stable to heat
Regional Availability
Other text information
Injection molding
PREPROCESSING
Pre/Post-processing, max. allowed water content: .04 %
Pre/Post-processing, Pre-drying, Temperature: 80 - 120 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 250 - 275 °C
injection molding, Melt temperature, recommended: 260 °C
injection molding, Mold temperature, range: 60 - 100 °C
injection molding, Mold temperature, recommended: 80 °C
Chemical Media Resistance
Acids
Acetic Acid (5% by mass) (23°C)
Application examples
Carrier frame, headrest, BMW
Frame, headlight
Handle, door
Housing, DeWALT hammer drill
Linkage, headrest, BMW
Mass air flow sensor
Plug, housing
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.