Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.
This is the free Material Data Center Datasheet of Ultramid® A3WG10 CR bk564 - PA66-GF50 - BASF
Material Data Center offers the following functions for Ultramid® A3WG10 CR bk564:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces
Check here, which other Ultramid A datasheets, application examples or technical articles are available in Material Data Center
Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our
disclaimer.
Processing/Physical Characteristics | dry / cond | Unit | Test Standard |
ISO Data |
Melt volume-flow rate, MVR |
10 / * |
cm³/10min |
ISO 1133 |
Temperature |
275 / * |
°C |
- |
Load |
5 / * |
kg |
- |
Molding shrinkage, parallel |
0.4 / * |
% |
ISO 294-4, 2577 |
Molding shrinkage, normal |
1.0 / * |
% |
ISO 294-4, 2577 |
Mechanical properties | dry / cond | Unit | Test Standard |
ISO Data |
Tensile Modulus |
16400 / 11500 |
MPa |
ISO 527 |
Stress at break |
230 / 160 |
MPa |
ISO 527 |
Strain at break |
2.5 / 4.1 |
% |
ISO 527 |
Flexural modulus, 23°C |
15500 / 11300 |
MPa |
ISO 178 |
Flexural modulus |
370 / 260 |
MPa |
ISO 178 |
Charpy impact strength, +23°C |
90 / 93 |
kJ/m² |
ISO 179/1eU |
Charpy impact strength, -30°C |
80 / 85 |
kJ/m² |
ISO 179/1eU |
Charpy notched impact strength, +23°C |
14 / 18 |
kJ/m² |
ISO 179/1eA |
Charpy notched impact strength, -30°C |
12 / 14 |
kJ/m² |
ISO 179/1eA |
Thermal properties | dry / cond | Unit | Test Standard |
ISO Data |
Melting temperature, 10°C/min |
260 / * |
°C |
ISO 11357-1/-3 |
Temp. of deflection under load, 1.80 MPa |
255 / * |
°C |
ISO 75-1/-2 |
Temp. of deflection under load, 0.45 MPa |
260 / * |
°C |
ISO 75-1/-2 |
Coeff. of linear therm. expansion, parallel |
16 / * |
E-6/K |
ISO 11359-1/-2 |
Coeff. of linear therm. expansion, normal |
80 / * |
E-6/K |
ISO 11359-1/-2 |
Electrical properties | dry / cond | Unit | Test Standard |
ISO Data |
Relative permittivity, 100Hz |
4.7 / 10.3 |
- |
IEC 62631-2-1 |
Relative permittivity, 1MHz |
4.3 / 4.9 |
- |
IEC 62631-2-1 |
Dissipation factor, 100Hz |
140 / 2230 |
E-4 |
IEC 62631-2-1 |
Dissipation factor, 1MHz |
180 / 730 |
E-4 |
IEC 62631-2-1 |
Volume resistivity |
4E12 / 2E9 |
Ohm*m |
IEC 62631-3-1 |
Surface resistivity |
* / 2E16 |
Ohm |
IEC 62631-3-2 |
Electric strength |
33 / 30 |
kV/mm |
IEC 60243-1 |
Comparative tracking index |
- / 600 |
- |
IEC 60112 |
Other properties | dry / cond | Unit | Test Standard |
Water absorption |
4 / * |
% |
Sim. to ISO 62 |
Humidity absorption |
1.2 / * |
% |
Sim. to ISO 62 |
Density |
1570 / - |
kg/m³ |
ISO 1183 |
Bulk density |
700 |
kg/m³ |
- |
Test specimen production | Value | Unit | Test Standard |
ISO Data |
Injection Molding, melt temperature |
300 |
°C |
ISO 294 |
Injection Molding, mold temperature |
100 |
°C |
ISO 294 |
Processing Recommendation Injection Molding | Value | Unit | Test Standard |
Melt temperature |
280 - 310 |
°C |
- |
Mold temperature |
80 - 100 |
°C |
- |
Processing Recommendation Extrusion | Value | Unit | Test Standard |
Melt temperature |
280 - 310 |
°C |
- |
Characteristics
Processing
Injection Molding, Other Extrusion
Delivery form
Pellets, Black
Features
Thermal Stability
Regional Availability
North America, Europe
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com