Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAKEEP® i4 3DF - PEEK - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAKEEP® i4 3DF:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vestakeep datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Processing/Physical Characteristicsdry / condUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 12 / * cm³/10min ISO 1133
Temperature 380 / * °C -
Load 5 / * kg -
Mechanical propertiesdry / condUnitTest Standard
ISO Data
Tensile Modulus 3500 / - MPa ISO 527
Tensile Strength 94 / - MPa ISO 527
Yield stress 94 / - MPa ISO 527
Yield strain 5 / - % ISO 527
Stress at break 76 / - MPa ISO 527
Charpy impact strength, +23°C N / - kJ/m² ISO 179/1eU
Charpy impact strength, -30°C N / - kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 6 / - kJ/m² ISO 179/1eA
Type of failure C / - - -
Charpy notched impact strength, -30°C 9.1 / - kJ/m² ISO 179/1eA
Type of failure C / - - -
Thermal propertiesdry / condUnitTest Standard
ISO Data
Melting temperature, 10°C/min 338 / * °C ISO 11357-1/-3
Glass transition temperature, 10°C/min 152 / * °C ISO 11357-1/-2
Temp. of deflection under load, 1.80 MPa 150 / * °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 205 / * °C ISO 75-1/-2
Vicat softening temperature, A 335 / * °C ISO 306
Vicat softening temperature, B 305 / * °C ISO 306
Burning behav. at thickness h V-0 / * class IEC 60695-11-10
Thickness tested 3.2 / * mm -
ASTM Data
Melting Temperature 338 °C ASTM D 3418
Other propertiesdry / condUnitTest Standard
Density 1300 / - kg/m³ ISO 1183
Density 1300 kg/m³ ASTM D 792
Characteristics
Processing
Additive Manufacturing
Delivery form
Monofilament, Natural Color
Special Characteristics
Heat stabilized or stable to heat
Features
Thermal Stability
Chemical Resistance
Acid Resistance, Alkali Resistance, General Chemical Resistance, Solvent Resistance, Grease Resistance, Hydrolytically Stable, Oil Resistance
Certifications
Medical Grade, Biocompatibility ISO 10993, US Pharmacopeia Class VI Approved
Applications
Medical
Regional Availability
Europe
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com