Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Vydyne® 47H BK03 - PA66 - Ascend

Material Data Center offers the following functions for Vydyne® 47H BK03:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vydyne datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
Vydyne 47H BK03 is general-purpose, medium impact-modified, heat stabilized PA66 resin. The product offers improved resistance to thermal degradation.
47H BK03 is recognized for all the processing and property advantages inherent to PA66 with the addition of improved impact strength. This resin offers a well balanced combination of engineering properties characterized by high melt point, good surface lubricity, abrasion resistance and resistance to many chemicals, machine and motor oils, solvents and gasoline.
Processing/Physical Characteristicsdry / condUnitTest Standard
ISO Data
Molding shrinkage, parallel 1.8 / * % ISO 294-4, 2577
Molding shrinkage, normal 1.6 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
ISO Data
Tensile Modulus 2800 / 1700 MPa ISO 527
Yield stress 60 / 45 MPa ISO 527
Stress at break 52 / 40 MPa ISO 527
Strain at break 22 / 60 % ISO 527
Flexural modulus, 23°C 2400 / 1000 MPa ISO 178
Flexural strength 75 / 26 MPa ISO 178
Charpy impact strength, +23°C N / N kJ/m² ISO 179/1eU
Charpy impact strength, -30°C N / N kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 16 / 55 kJ/m² ISO 179/1eA
Charpy notched impact strength, -30°C 11 / 17 kJ/m² ISO 179/1eA
Izod notched impact strength, +23°C 15 / 44 kJ/m² ISO 180/1A
Izod notched impact strength 12 / 18 kJ/m² ISO 180/1A
Temperature -30 °C -
Thermal propertiesdry / condUnitTest Standard
ISO Data
Melting temperature, 10°C/min 260 / * °C ISO 11357-1/-3
Temp. of deflection under load, 1.80 MPa 64 / * °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 185 / * °C ISO 75-1/-2
Coeff. of linear therm. expansion, parallel 111 / * E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion, normal 136 / * E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB / * class IEC 60695-11-10
Thickness tested 1.5 / * mm -
Burning Behav. at thickness h HB / * class IEC 60695-11-10
Thickness tested 0.8 / * mm -
Glow Wire Flammability Index (GWFI) 700 °C IEC 60695-2-12
GWFI - thickness tested (1) 0.75 mm -
Glow Wire Flammability Index (GWFI) 775 °C IEC 60695-2-12
GWFI - thickness tested (2) 1.5 mm -
Glow Wire Flammability Index (GWFI) 700 °C IEC 60695-2-12
GWFI - thickness tested (3) 3 mm -
Glow Wire Ignition Temperature (GWIT) 725 °C IEC 60695-2-13
GWIT - thickness tested (1) 0.75 mm -
Glow Wire Ignition Temperature (GWIT) 800 °C IEC 60695-2-13
GWIT - thickness tested (2) 1.5 mm -
Glow Wire Ignition Temperature (GWIT) 725 °C IEC 60695-2-13
GWIT - thickness tested (3) 3 mm -
ASTM Data
UL 94 Flame rating HB - UL 94
Thickness tested 0.75 mm -
Electrical propertiesdry / condUnitTest Standard
ISO Data
Volume resistivity 1E9 / - Ohm*m IEC 62631-3-1
Electric strength 12 / - kV/mm IEC 60243-1
Comparative tracking index 525 / - - IEC 60112
ASTM Data
Arc Resistance 90 / - s ASTM D 495
Other propertiesdry / condUnitTest Standard
Water absorption 1.2 / * % Sim. to ISO 62
Humidity absorption 2.3 / * % Sim. to ISO 62
Density 1100 / - kg/m³ ISO 1183
Processing Recommendation Injection MoldingValueUnitTest Standard
Pre-drying - Temperature 80 °C -
Pre-drying - Time 4 h -
Melt temperature 285 - 305 °C -
Mold temperature 65 - 95 °C -
Zone 1 280 - 310 °C -
Zone 2 280 - 310 °C -
Zone 3 280 - 310 °C -
Nozzle temperature 280 - 310 °C -
Characteristics
Processing
Injection Molding
Delivery form
Pellets, Black
Additives
Lubricants
Special Characteristics
High impact or impact modified, Heat stabilized or stable to heat
Chemical Resistance
General Chemical Resistance, Solvent Resistance, Oil Resistance
Applications
Automotive, Electrical and Electronical, General Purpose
Regional Availability
North America, Europe, Asia Pacific
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.