Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of DOWLEX™ 2645 - (PE-LLD) - The Dow Chemical Company

Material Data Center offers the following functions for DOWLEX™ 2645:
unit conversion, PDF datasheet print, comparison with other plastics

Check here, which other Dowlex datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Processing/Physical CharacteristicsValueUnitTest Standard
ISO Data
Melt flow index, MFI 0.85 g/10min ISO 1133
Temperature 190 °C -
Load 2.16 kg -
Thermal propertiesValueUnitTest Standard
ISO Data
Coeff. of linear therm. expansion, parallel 39 E-6/K ISO 11359-1/-2
ASTM Data
Vicat Temperature 107 °C ASTM D 1525
Optical propertiesValueUnitTest Standard
ISO Data
Haze 10 - ISO 14782
ASTM Data
Gloss 59 - ASTM D 2457
Other propertiesValueUnitTest Standard
Density 918 kg/m³ ASTM D 792
Film PropertiesValueUnitTest Standard
ISO Data
Stress at yield, parallel 7.5 MPa ISO 527-3
Stress at yield, normal 6.3 MPa ISO 527-3
Stress at break, parallel 39 MPa ISO 527-3
Stress at break, normal 40 MPa ISO 527-3
Maximum strain, parallel 560 % ISO 527-3
Maximum strain, normal 670 % ISO 527-3
Dart drop A 480 g ISO 7765-1
Type of extrusion blown - -
Thickness of specimen 0.05 mm -
Characteristics
Processing
Blown Film Extrusion, Film Extrusion
Delivery form
Pellets, White
Features
Low Odor
Certifications
Food contact, Food approval 10/2011, Food contact notification (FCN)
Regional Availability
Europe, Near East/Africa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.