Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.
This is the free Material Data Center Datasheet of Pebax® Rnew® 35R53 SP 01 - TPA - ARKEMA
unit conversion, PDF datasheet print, comparison with other plastics
Check here, which other Pebax datasheets, application examples or technical articles are available in Material Data Center
Main applications:
- Flexible injected parts
Packaging:
This grade is delivered dried in sealed packaging (25 kg bags) ready to be processed.
Shelf Life:
Two years from the delivery. For any use above this limit, please refer to our technical services.
Processing/Physical Characteristics | dry / cond | Unit | Test Standard | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
ISO Data | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
Molding shrinkage, parallel | 0.1 / * | % | ISO 294-4, 2577 | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
Molding shrinkage, normal | 1.0 / * | % | ISO 294-4, 2577 |
Mechanical properties | dry / cond | Unit | Test Standard | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
ISO Data | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
Tensile Modulus | - / 40 | MPa | ISO 527 | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
Stress at 50% strain | - / 5 | MPa | ISO 527 | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
Strain at break | - / >50 | % | ISO 527 | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
Stress at break TPE | 30 / * | MPa | ISO 527 | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
Strain at break TPE | >300 / * | % | ISO 527 | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
Shore D hardness | 25 / * | - | ISO 7619-1 |
Thermal properties | dry / cond | Unit | Test Standard | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
ISO Data | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
Melting temperature, 10°C/min | 135 / * | °C | ISO 11357-1/-3 |
Other properties | dry / cond | Unit | Test Standard |
Water absorption | 1.3 / * | % | Sim. to ISO 62 |
Humidity absorption | 0.5 / * | % | Sim. to ISO 62 |
Density | 1020 / 1020 | kg/m³ | ISO 1183 |
Biobased content | 29 | % | - |
Processing Recommendation Injection Molding | Value | Unit | Test Standard |
Pre-drying - Temperature | 55 - 65 | °C | - |
Pre-drying - Time | 4 - 8 | h | - |
Melt temperature | 180 - 260 | °C | - |
Mold temperature | 10 - 30 | °C | - |
Processing conditions (injection molding):
- Typical melt temperature (Min / Recommended / Max) : 180°C / 210°C / 260°C.
- Typical mold temperature : 10 – 30°C.
- Drying time and temperature (only necessary for bags opened for more than two hours) : 4-8 hours at 55-65°C.
Processing conditions (extrusion):
- Typical melt temperature (Min / Recommended / Max): 190°C / 205°C / 220°C.- Drying time and temperature (only necessary for bags opened for more than two hours): 4-8 hours at 55-65°C.