Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Rilsan® Clear G820 Rnew® - PA* - ARKEMA

Material Data Center offers the following functions for Rilsan® Clear G820 Rnew®:
unit conversion, PDF datasheet print, comparison with other plastics

Check here, which other Rilsan datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
PA,,MHT,C14-020

Rilsan® Clear  G820 Rnew® is a high performance transparent polyamide with outstanding chemical resistance and stress cracking resistance.This grade has been designed for injection molding applications.

According to ASTM D6866, the biobased carbon content is measured at 62%.



Main applications:
  • Optic
  • Electonics
  • Domestic appliances

Packaging:
This grade is delivered dried in sealed packaging (25 kg bags) ready to be processed.

Shelf Life:
Two years from the delivery. For any use above this limit,  please refer to our technical services.
Processing/Physical Characteristicsdry / condUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 8 / * cm³/10min ISO 1133
Temperature 275 / * °C -
Load 2.16 / * kg -
Molding shrinkage, parallel 0.6 / * % ISO 294-4, 2577
Molding shrinkage, normal 0.7 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
ISO Data
Tensile Modulus - / 1665 MPa ISO 527
Yield stress - / 66 MPa ISO 527
Yield strain - / 7 % ISO 527
Nominal strain at break - / >50 % ISO 527
Charpy notched impact strength, +23°C - / 6 kJ/m² ISO 179/1eA
Charpy notched impact strength, -30°C - / 9 kJ/m² ISO 179/1eA
Shore D hardness 76 / * - ISO 7619-1
Thermal propertiesdry / condUnitTest Standard
ISO Data
Glass transition temperature, 10°C/min 101 / * °C ISO 11357-1/-2
Temp. of deflection under load, 1.80 MPa 73 / * °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 85 / * °C ISO 75-1/-2
Other propertiesdry / condUnitTest Standard
Water absorption 2.45 / * % Sim. to ISO 62
Humidity absorption 1.16 / * % Sim. to ISO 62
Density 1000 / 1000 kg/m³ ISO 1183
Biobased content 60 % -
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Special Characteristics
Transparent
Chemical Resistance
General Chemical Resistance, Environmental Stress Crack Resistance
Certifications
Contains renewable resources
Applications
Electrical and Electronical
Regional Availability
Other text information
Injection molding
Processing conditions:
- Typical melt temperature  (Min / Recommaneded / Max)  : 260°C / 280°C / 300°C
- Typical mold temperature  : 20 - 80 °C
- Dyring time and temperature (only for bags opened for more than two hours): 4 - 6 hours at 80°C

 

Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.