Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultradur® B 6550 - PBT - BASF

Material Data Center offers the following functions for Ultradur® B 6550:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultradur datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
High viscosity extrusion grade of fibre optical cable sheaths for semi-finished products, profile and hollow rods in technical applications.

Abbreviated designation according to ISO 1043-1: PBT
Processing/Physical CharacteristicsValueUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 9 cm³/10min ISO 1133
Temperature 250 °C -
Load 2.16 kg -
Molding shrinkage, parallel 1.7 % ISO 294-4, 2577
Molding shrinkage, normal 2.1 % ISO 294-4, 2577
ASTM Data
Mold Shrinkage, MD 0.015 mm/mm ASTM D 955
Mechanical propertiesValueUnitTest Standard
ISO Data
Tensile Modulus 2400 MPa ISO 527
Yield stress 54 MPa ISO 527
Yield strain 3.5 % ISO 527
Nominal strain at break >50 % ISO 527
Tensile creep modulus, 1h 1800 MPa ISO 899-1
Tensile creep modulus, 1000h 1100 MPa ISO 899-1
Charpy impact strength, +23°C N kJ/m² ISO 179/1eU
Charpy impact strength, -30°C 250 kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 6 kJ/m² ISO 179/1eA
Charpy notched impact strength, -30°C 3.5 kJ/m² ISO 179/1eA
ASTM Data
Tensile Modulus 2482 MPa ASTM D 638
Tensile Strength at Yield 60 MPa ASTM D 638
Elongation at Yield 3.5 % ASTM D 638
Thermal propertiesValueUnitTest Standard
ISO Data
Melting temperature, 10°C/min 223 °C ISO 11357-1/-3
Temp. of deflection under load, 1.80 MPa 55 °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 135 °C ISO 75-1/-2
Coeff. of linear therm. expansion, parallel 110 E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion, normal 110 E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB class IEC 60695-11-10
Thickness tested 1.5 mm -
Burning Behav. at thickness h HB class IEC 60695-11-10
Thickness tested 0.8 mm -
ASTM Data
DTUL @ 66 psi 135 °C ASTM D 648
DTUL @ 264 psi 53.9 °C ASTM D 648
Melting Temperature 223 °C ASTM D 3418
Electrical propertiesValueUnitTest Standard
ISO Data
Relative permittivity, 100Hz 3.3 - IEC 62631-2-1
Relative permittivity, 1MHz 3.3 - IEC 62631-2-1
Dissipation factor, 100Hz 10 E-4 IEC 62631-2-1
Dissipation factor, 1MHz 200 E-4 IEC 62631-2-1
Volume resistivity >1E13 Ohm*m IEC 62631-3-1
Surface resistivity 1E13 Ohm IEC 62631-3-2
Comparative tracking index 600 - IEC 60112
Other propertiesValueUnitTest Standard
Water absorption 0.5 % Sim. to ISO 62
Humidity absorption 0.25 % Sim. to ISO 62
Density 1300 kg/m³ ISO 1183
Density 1300 kg/m³ ASTM D 792
Material specific propertiesValueUnitTest Standard
ISO Data
Viscosity number 160 cm³/g ISO 307, 1157, 1628
Processing Recommendation Injection MoldingValueUnitTest Standard
Pre-drying - Temperature 80 - 120 °C -
Pre-drying - Time 4 h -
Processing humidity ≤0.04 % -
Melt temperature 250 - 275 °C -
Mold temperature 40 - 80 °C -
Diagrams
Viscosity-shear rate , Ultradur® B 6550, PBT, BASF
Shearstress-shear rate , Ultradur® B 6550, PBT, BASF
Stress-strain , Ultradur® B 6550, PBT, BASF
Secant modulus-strain , Ultradur® B 6550, PBT, BASF
Stress-strain (isochronous) 23°C, Ultradur® B 6550, PBT, BASF
Creep modulus-time 23°C, Ultradur® B 6550, PBT, BASF
Creep curve 23°C, Ultradur® B 6550, PBT, BASF
Tensile modulus-temperature , Ultradur® B 6550, PBT, BASF
Characteristics
Processing
Injection Molding, Film Extrusion, Profile Extrusion, Sheet Extrusion, Other Extrusion
Delivery form
Pellets, Natural Color
Special Characteristics
Light stabilized or stable to light, U.V. stabilized or stable to weather, Heat stabilized or stable to heat
Regional Availability
Other text information
Injection molding
PREPROCESSING
Pre/Post-processing, max. allowed water content: .04 %
Pre/Post-processing, Pre-drying, Temperature: 80 - 120 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 250 - 275 °C
injection molding, Melt temperature, recommended: 260 °C
injection molding, Mold temperature, range: 40 - 80 °C
injection molding, Mold temperature, recommended: 60 °C
injection molding, Dwell time, thermoplastics: 10 min
Other extrusion
PREPROCESSING
Pre/Post-processing, max. allowed water content: .04 %
Pre/Post-processing, Pre-drying, Temperature: 80 - 120 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
Extrusion, Prepreg, Melt temperature: 230 - 250 °C
Extrusion, Pipes, Melt temperature: 230 - 260 °C
Extrusion, cable sheathing, Melt temperature: 230 - 260 °C
Profile extrusion
PREPROCESSING
Pre/Post-processing, max. allowed water content: .04 %
Pre/Post-processing, Pre-drying, Temperature: 80 - 120 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
Extrusion, Profiles, Melt temperature: 230 - 260 °C
Sheet extrusion
PREPROCESSING
Pre/Post-processing, max. allowed water content: .04 %
Pre/Post-processing, Pre-drying, Temperature: 80 - 120 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
Extrusion, Plates, Melt temperature: 230 - 250 °C
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.