Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAKEEP® 4000 P - PEEK - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAKEEP® 4000 P:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vestakeep datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
Unreinforced, high-viscosity polyether ether ketone powder

VESTAKEEP® 4000 P is an unreinforced, high-viscosity polyether ether ketone powder. The product is suitable for the manufacture of compounds or it can be used as scatter-powder for the manufacture of composites.

The semi-crystalline polymer features superior thermal and chemical resistance. VESTAKEEP® 4000 P is of low flammability.

VESTAKEEP® 4000 P is supplied as powder in boxes with moisture-proof polyethylene liners.

Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at temperatures not exceeding 30°C.

Pigmentation may affect the values.

For information about processing of VESTAKEEP® 4000 P, please follow the general recommendations in our brochure “VESTAKEEP® High Performance in Powder Form Polyether Ether Ketone Powders“.

The values presented are typical or average values, they do not constitute a specification. 

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM OR VISIT OUR PRODUCT AT WWW.INDUSTRIAL.VESTAKEEP.COM
Processing/Physical CharacteristicsValueUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 11 cm³/10min ISO 1133
Temperature 380 °C -
Load 5 kg -
Mechanical propertiesValueUnitTest Standard
ISO Data
Tensile Modulus 3600 MPa ISO 527
Yield stress 93 MPa ISO 527
Yield strain 5 % ISO 527
Nominal strain at break 30 % ISO 527
Charpy impact strength, +23°C N kJ/m² ISO 179/1eU
Charpy impact strength, -30°C N kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 7 kJ/m² ISO 179/1eA
Type of failure C - -
Charpy notched impact strength, -30°C 6 kJ/m² ISO 179/1eA
Type of failure C - -
Thermal propertiesValueUnitTest Standard
ISO Data
Melting temperature, 10°C/min 337 °C ISO 11357-1/-3
Glass transition temperature, 10°C/min 152 °C ISO 11357-1/-2
Temp. of deflection under load, 1.80 MPa 150 °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 205 °C ISO 75-1/-2
Vicat softening temperature, B 305 °C ISO 306
Other propertiesValueUnitTest Standard
Density 1300 kg/m³ ISO 1183
Test specimen productionValueUnitTest Standard
ISO Data
Injection Molding, melt temperature 380 °C ISO 294
Injection Molding, mold temperature 180 °C ISO 294
Injection Molding, injection velocity 200 mm/s ISO 294
Characteristics
Processing
Coating, Transfer Molding
Delivery form
Powder
Features
Thermal Stability
Chemical Resistance
General Chemical Resistance
Regional Availability
North America, Europe, Asia Pacific, South and Central America, Near East/Africa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.