Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAKEEP® DC 4420 G - PEEK - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAKEEP® DC 4420 G:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vestakeep datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
White pigmented polyether ether ketone for dental applications

VESTAKEEP® DC4420 G white pigmented polyether ether ketone for dental applications high viscosity polyether ether ketone (PEEK) resin that is especially designed for removable and fixed dentures, crowns and bridges.

Biocompatibility of VESTAKEEP® Dental
For VESTAKEEP® DC4420 G, biocompatibility has been tested according to ISO 10993-1 recommendations for permanent mucous membrane contact. The compound composition is optimised for high biocompatibility and superior mechanical, thermal and chemical resistance.
 
Biocompatibility test reports available for VESTAKEEP® DC4420 G
Standard Description
ISO 10993-03 Genotoxicity: Salmonella Typhimurium Reverse Mutation Test (Ames Test)
ISO 10993-05 Cytotoxicity: Quantitative Growth Inhibition Test
ISO 10993-10 Irritation: Intracutaneous Reactivity
ISO 10993-10 Sensitization: Local Lymph Node Assay
ISO 10993-11 Acute Systemic Toxicity
ISO 10993-11 Subacute / Subchronic Toxicity 14 days
ISO 10993-18 Extraction Tests
USP Class VI Acute Systemic Toxicity Intracutaneous Reactivity Muscle Implantation

Processing of VESTAKEEP® Dental
VESTAKEEP® DC4420 G can be processed by common melt processing techniques like injection molding and extrusion.
For injection molding, we recommend a melt temperature in the 380°C to 400°C range. The mold temperature should be within 160°C to 200°C, preferably 180°C.

Delivery of VESTAKEEP® Dental
VESTAKEEP® DC4420 G is supplied as granules in 25 kg boxes with moisture-proof polyethylene liners.

The values presented are typical or average values, they do not constitute a specification. 

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM
OR VISIT OUR PRODUCT AT  WWW.EVONIK.COM/MEDICAL-TECHNOLOGY 


 
Processing/Physical CharacteristicsValueUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 11 cm³/10min ISO 1133
Temperature 380 °C -
Load 5 kg -
Molding shrinkage, parallel 1.0 % ISO 294-4, 2577
Molding shrinkage, normal 1.1 % ISO 294-4, 2577
Mechanical propertiesValueUnitTest Standard
ISO Data
Tensile Modulus 4100 MPa ISO 527
Yield stress 95 MPa ISO 527
Yield strain 4.8 % ISO 527
Nominal strain at break 18 % ISO 527
Charpy impact strength, +23°C N kJ/m² ISO 179/1eU
Charpy impact strength, -30°C N kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 6.8 kJ/m² ISO 179/1eA
Type of failure C - -
Charpy notched impact strength, -30°C 6 kJ/m² ISO 179/1eA
Type of failure C - -
Thermal propertiesValueUnitTest Standard
ISO Data
Melting temperature, 10°C/min 336 °C ISO 11357-1/-3
Glass transition temperature, 10°C/min 155 °C ISO 11357-1/-2
Temp. of deflection under load, 1.80 MPa 155 °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 210 °C ISO 75-1/-2
Vicat softening temperature, B 305 °C ISO 306
Coeff. of linear therm. expansion, parallel 45 E-6/K ISO 11359-1/-2
Other propertiesValueUnitTest Standard
Water absorption 0.4 % Sim. to ISO 62
Density 1490 kg/m³ ISO 1183
Test specimen productionValueUnitTest Standard
ISO Data
Injection Molding, melt temperature 385 °C ISO 294
Injection Molding, mold temperature 180 °C ISO 294
Injection Molding, injection velocity 200 mm/s ISO 294
Characteristics
Processing
Injection Molding, Other Extrusion
Delivery form
Pellets, White
Features
Thermal Stability
Chemical Resistance
General Chemical Resistance
Certifications
Medical Grade, Biocompatibility ISO 10993, US Pharmacopeia Class VI Approved
Applications
Medical
Regional Availability
North America, Europe, Asia Pacific, South and Central America, Near East/Africa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.