Caracteristicas de procesamiento y fisicas | Valor | Unidades | Método de ensayo |
ISO Data |
Indice de fluidez volumétrico, MVR |
18 |
cm³/10min |
ISO 1133 |
Temperatura |
190 |
°C |
- |
Carga |
2.16 |
kg |
- |
Other Standards[S] |
Contracción posterior al moldeo, paralelo |
3.0 |
% |
|
S: | These properties are reported by the producer according standards that are different to our defaults. |
Propiedades mecánicas | Valor | Unidades | Método de ensayo |
ISO Data |
Dureza Shore A |
88 |
- |
ISO 7619-1 |
Other Standards[S] |
Módulo de flexión, 23°C |
27 |
MPa |
ISO 6721-1 |
Modulo de Flexión |
72 |
MPa |
ISO 6721-1 |
Modulo de Flexión - Temperatura |
60 |
°C |
- |
S: | These properties are reported by the producer according standards that are different to our defaults. |
Propiedades térmicas | Valor | Unidades | Método de ensayo |
ISO Data |
Temperatura de fusión, 10°C/min |
160 |
°C |
ISO 11357-1/-3 |
Temp. reblandecimiento Vicat, A |
90 |
°C |
ISO 306 |
Other Standards[S] |
Temp. de transición vítrea, 10°C/min |
-13.6 |
°C |
ISO 6721-1 |
S: | These properties are reported by the producer according standards that are different to our defaults. |
Otras propiedades | Valor | Unidades | Método de ensayo |
Densidad |
1200 |
kg/m³ |
ISO 1183 |
Bulk density |
457 |
kg/m³ |
- |
3D Data | Valor | Unidades | Método de ensayo |
Other Standards[S] |
Esfuerzo de tracción, flat |
20[1] |
MPa |
DIN 53504 |
Esfuerzo de tracción, upright |
15[2] |
MPa |
DIN 53504 |
Alargamiento a rotura, flat |
520[1] |
% |
DIN 53504 |
Alargamiento a rotura, upright |
500[2] |
% |
DIN 53504 |
1: | XY-direction | 2: | ZX-direction | S: | These properties are reported by the producer according standards that are different to our defaults. |
Características
Procesamiento y forma de entrega
Additive Manufacturing, Sinterizado por láser
Forma de suministro
Polvo, Blanco
Applicaciones
Equipos deportivos
Disponibilidad regional
Norteamérica, Europa, Asia Pacifico, América del Sur y Centroaméric
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com