Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Pebax® 3533 SP 01 - TPA - ARKEMA

Material Data Center offers the following functions for Pebax® 3533 SP 01:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Pebax datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Texto del producto
Polyether block amide Pebax® 3533 SP 01 resin is a thermoplastic elastomer made of flexible polyether and rigid polyamide.
This SP grade has been developed to be heat and UV resistant.


Main applications:
  • Flexible injected parts
  • High performance power trasmission belts
  • Silent gears
  • Toy component


Packaging:

This grade is delivered dried in sealed packaging (25 kg bags) ready to be processed.

Shelf Life:
Two years from the delivery. For any use above this limit, please refer to our technical services.
Propiedades mecánicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Módulo de tracción 19 / 18 MPa ISO 527
Esfuerzo a 50% de alarg. 4 / 4 MPa ISO 527
Alargamiento a rotura >50 / >50 % ISO 527
Tensión a 10% alargamiento 2 / * MPa ISO 527
Tensión a 100% alargamiento 6 / * MPa ISO 527
Resistencia a la tracción TPE 39 / * MPa ISO 527
Alargamiento a rotura TPE >300 / * % ISO 527
Deformación permanente por compresión a 23°C, 24h 22 / * % ISO 815
Resistencia al desgarro 50 / * kN/m ISO 34-1
Resistencia a la abrasión 64 / * mm³ ISO 4649
Dureza Shore A 80 / * - ISO 7619-1
Dureza Shore D 25 / * - ISO 7619-1
Propiedades térmicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Temperatura de fusión, 10°C/min 144 / * °C ISO 11357-1/-3
Temp. de transición vítrea, 10°C/min -65 / * °C ISO 11357-1/-2
Estabilidad al calor, 0.45 MPa 46 / * °C ISO 75-1/-2
Coef.de expansión térmica lineal, paralelo 210 / * E-6/K ISO 11359-1/-2
Propiedades eléctricasSeco / CondUnidadesMétodo de ensayo
ISO Data
Constante dieléctrica, 100Hz 6 / - - IEC 62631-2-1
Constante dieléctrica, 1MHz 6 / - - IEC 62631-2-1
Factor de pérdidas dieléctricas, 100Hz 310 / - E-4 IEC 62631-2-1
Factor de pérdidas dieléctricas, 1MHz 434 / - E-4 IEC 62631-2-1
Resistividad volumétrica específica 3.2E10 / - Ohm*m IEC 62631-3-1
Resistividad superficial específica * / 3E12 Ohm IEC 62631-3-2
Resistencia dieléctrica 33.5 / - kV/mm IEC 60243-1
Indice comparativo de linea de fuga * / 600 - IEC 60112
Otras propiedadesSeco / CondUnidadesMétodo de ensayo
Absorción de agua 1.2 / * % Sim. to ISO 62
Absorción de humedad 0.4 / * % Sim. to ISO 62
Densidad 1000 / 1000 kg/m³ ISO 1183
Recomendación para procesamiento Moldeo por inyecciónValorUnidadesMétodo de ensayo
Temperatura de pre-secado 55 - 65 °C -
Tiempo de pre-secado 4 - 8 h -
Temperatura de la masa 180 - 240 °C -
Temperatura del molde 10 - 30 °C -
Funciones
Viscosidad-velocidad de cizallamiento , Pebax® 3533 SP 01, TPA, ARKEMA
Tensión de cizalla-velocidad de cizalla , Pebax® 3533 SP 01, TPA, ARKEMA
Esfuerzo-alargamiento , Pebax® 3533 SP 01 (Seco), TPA, ARKEMA
Módulo secante-alargamiento , Pebax® 3533 SP 01 (Seco), TPA, ARKEMA
Esfuerzo-alargamiento (isocrono) 23°C, Pebax® 3533 SP 01 (Seco), TPA, ARKEMA
Módulo de plastodeformación-tiempo 23°C, Pebax® 3533 SP 01 (Seco), TPA, ARKEMA
Curva de creep 23°C, Pebax® 3533 SP 01 (Seco), TPA, ARKEMA
Volumen especifico-temperatura (pvT) , Pebax® 3533 SP 01, TPA, ARKEMA
Características
Procesamiento y forma de entrega
Moldeo por inyección, Extrusion del film, Extrusión de perfiles, Otros tipos de extrusión, Transfer Molding, Colado, Termoconformación
Forma de suministro
Sémola
Aditivos
Lubricante, Agente antibloqueo
Características especiales
Galvanizable, Estable a la luz, Estable contra rayos U.V./interperie, Estable contra el calor
Disponibilidad regional
Demás información
Moldeo por inyección

Processing conditions:

- Typical melt temperature (Min / Recommended / Max) : 180°C / 210°C / 240°C.
- Typical mold temperature : 10 – 30°C.
- Drying time and temperature (only necessary for bags opened for more than two hours) : 4-8 hours at 55-65°C
Otros tipos de extrusión

Processing conditions:

- Typical melt temperature (Min / Recommended / Max) : 190°C / 205°C / 220°C.
- Drying time and temperature (only necessary for bags opened for more than two hours) : 4-8 hours at 55-65°C.
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.