Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultramid® B3G4 - PA6-GF20 - BASF

Material Data Center offers the following functions for Ultramid® B3G4:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Ultramid B datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Texto del producto
20% glass reinforced nylon 6 injection molding compound possessing a balance of engineering properties combined with excellent processability and surface aesthetics. It is ideally suited for more demanding performance applications such as safety helmet parts, washers, gears, engine and motor parts, chutes.
Propiedades mecánicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Módulo de tracción 6700 / - MPa ISO 527
Resistencia a la tracción 140 / - MPa ISO 527
Alargamiento a rotura 4 / - % ISO 527
Módulo de flexión, 23°C 5700 / - MPa ISO 178
Resistencia al impacto Charpy, +23°C 60 / - kJ/m² ISO 179/1eU
Resistencia al impacto Charpy c/entalla, +23°C 8 / - kJ/m² ISO 179/1eA
Propiedades térmicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Temperatura de fusión, 10°C/min 220 / * °C ISO 11357-1/-3
Estabilidad al calor, 1.80 MPa 200 / * °C ISO 75-1/-2
Estabilidad al calor, 0.45 MPa 215 / * °C ISO 75-1/-2
Coef.de expansión térmica lineal, paralelo 25 / * E-6/K ISO 11359-1/-2
Coef.de expansión térmica lineal, normal 110 / * E-6/K ISO 11359-1/-2
Propiedades eléctricasSeco / CondUnidadesMétodo de ensayo
ISO Data
Resistividad volumétrica específica >1E13 / - Ohm*m IEC 62631-3-1
Otras propiedadesSeco / CondUnidadesMétodo de ensayo
Absorción de agua 7.6 / * % Sim. to ISO 62
Absorción de humedad 2.2 / * % Sim. to ISO 62
Densidad 1280 / * kg/m³ ISO 1183
Bulk density 700 kg/m³ -
Propiedades específicas del materialSeco / CondUnidadesMétodo de ensayo
ISO Data
Indice de viscosidad 145 / * cm³/g ISO 307, 1157, 1628
Recomendación para procesamiento Moldeo por inyecciónValorUnidadesMétodo de ensayo
Temperatura de pre-secado 80 °C -
Tiempo de pre-secado 4 h -
Humedad de procesamiento ≤0.15 % -
Temperatura de la masa 270 - 295 °C -
Temperatura del molde 80 - 95 °C -
Características
Procesamiento y forma de entrega
Moldeo por inyección
Forma de suministro
Sémola
Aditivos
Desmoldeante
Disponibilidad regional
Norteamérica, Europa
Demás información
Moldeo por inyección
PREPROCESSING
Pre/Post-processing, max. allowed water content: .15 %
Pre/Post-processing, Pre-drying, Temperature: 80 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 270 - 290 °C
injection molding, Melt temperature, recommended: 280 °C
injection molding, Mold temperature, range: 80 - 90 °C
injection molding, Mold temperature, recommended: 80 °C
injection molding, Dwell time, thermoplastics: 10 min

PREPROCESSING
Max. Water content: 0.12%
Product is supplied in sealed containers and drying prior to molding is not required. If drying becomes necessary, a dehumidifying or desiccant dryer operating at 80 °C (176 °F) is recommended. Drying time is dependent on moisture level.
Further information concerning safe handling procedures can be obtained from the Material Safety Data Sheet. Alternatively, please contact your BASF representative.

PROCESSING
Melt Temperature 270-295 °C (518-563 °F)
Mold Temperature 80-95 °C (176-203 °F)
Injection and Packing Pressure 35-125 bar (500-1500 psi)

This product can be processed over a wide range of mold temperatures; however, for applications where aesthetics are critical, a mold surface temperature of 80-95 °C (176-203 °F) is required.

Injection pressure controls the filling of the part and should be applied for 90% of ram travel. Packing pressure affects the final part and can be used effectively in controlling sink marks and shrinkage. It should be applied and maintained until the gate area is completely frozen off.

Back pressure can be utilized to provide uniform melt consistency and reduce trapped air and gas. A maximum of 3.5 bar (50 psi) is recommended to minimize glass fiber breakage.

Fast fill rates are recommended to insure uniform melt delivery to the cavity and prevent premature freezing. Surface appearance is directly affected by injection rate.
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.