Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultrason® E 2010 C6 - PESU-CF30 - BASF

Material Data Center offers the following functions for Ultrason® E 2010 C6:
unit conversion, PDF datasheet print, comparison with other plastics, application examples, parameters for material models, CAE Interfaces

Check here, which other Ultrason E datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Texto del producto
Medium viscosity injection moulding grade with high rigidity and strength, 30 % carbon fiber reinforced.
Abbreviated designation according to ISO 1043: PESU-CF
Caracteristicas de procesamiento y fisicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Indice de fluidez volumétrico, MVR 15 / * cm³/10min ISO 1133
Temperatura 360 / * °C -
Carga 10 / * kg -
Contracción posterior al moldeo, paralelo 0.1 / * % ISO 294-4, 2577
Contracción posterior al moldeo, normal 0.3 / * % ISO 294-4, 2577
Propiedades mecánicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Módulo de tracción - / 22000 MPa ISO 527
Resistencia a la tracción - / 185 MPa ISO 527
Alargamiento a rotura - / 1.5 % ISO 527
Resistencia al impacto Charpy, +23°C - / 40 kJ/m² ISO 179/1eU
Resistencia al impacto Charpy, -30°C - / 40 kJ/m² ISO 179/1eU
Resistencia al impacto Charpy c/entalla, +23°C - / 7.5 kJ/m² ISO 179/1eA
Resistencia al impacto Charpy c/entalla, -30°C - / 6.5 kJ/m² ISO 179/1eA
Propiedades térmicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Temp. de transición vítrea, 10°C/min 225 / * °C ISO 11357-1/-2
Estabilidad al calor, 1.80 MPa 225 / * °C ISO 75-1/-2
Estabilidad al calor, 0.45 MPa 230 / * °C ISO 75-1/-2
Coef.de expansión térmica lineal, paralelo 4 / * E-6/K ISO 11359-1/-2
Coef.de expansión térmica lineal, normal 37 / * E-6/K ISO 11359-1/-2
Combustibilidad según índice de oxigeno 51.9 / * % ISO 4589-1/-2
Propiedades eléctricasSeco / CondUnidadesMétodo de ensayo
ISO Data
Resistividad superficial específica * / 1000 Ohm IEC 62631-3-2
Otras propiedadesSeco / CondUnidadesMétodo de ensayo
Absorción de agua 1.7 / * % Sim. to ISO 62
Absorción de humedad 0.6 / * % Sim. to ISO 62
Densidad 1470 / - kg/m³ ISO 1183
Propiedades específicas del materialSeco / CondUnidadesMétodo de ensayo
ISO Data
Indice de viscosidad 56 / * cm³/g ISO 307, 1157, 1628
Recomendación para procesamiento Moldeo por inyecciónValorUnidadesMétodo de ensayo
Temperatura de pre-secado 140 °C -
Tiempo de pre-secado 4 h -
Humedad de procesamiento ≤0.02 % -
Temperatura de la masa 350 - 390 °C -
Temperatura del molde 150 - 190 °C -
Funciones
Esfuerzo-alargamiento (isocrono) 23°C, Ultrason® E 2010 C6 (Cond), PESU-CF30, BASF
Módulo de plastodeformación-tiempo 23°C, Ultrason® E 2010 C6 (Cond), PESU-CF30, BASF
Curva de creep 23°C, Ultrason® E 2010 C6 (Cond), PESU-CF30, BASF
Volumen especifico-temperatura (pvT) , Ultrason® E 2010 C6, PESU-CF30, BASF
Características
Procesamiento y forma de entrega
Moldeo por inyección, Extrusión de perfiles, Extrusión de láminas, Otros tipos de extrusión
Forma de suministro
Sémola
Características especiales
Conductividad eléctrica aumentada, Antiestático
Disponibilidad regional
Demás información
Moldeo por inyección
PREPROCESSING
Pre/Post-processing, max. allowed water content: .02 %
Pre/Post-processing, Pre-drying, Temperature: 140 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 350 - 390 °C
injection molding, Melt temperature, recommended: 370 °C
injection molding, Mold temperature, range: 150 - 190 °C
injection molding, Mold temperature, recommended: 170 °C
injection molding, Dwell time, thermoplastics: 10 min

Pretreatment
Drying temperature: 130 - 150°C
Drying time: minimum 4h
recommended dryer: vaccum or dry air dryer
maximum moisture: 0,02 - 0,05%

Ultrason® can be injection molded by any type of machinery on the market, provided that the plasticizing unit and the mold temperature control system have been configured appropriately. The machinery manufacturer must be consulted if any doubts exist on the ability of various parts to withstand the high temperatures required (e.g. barrel, barrel head, bolted connections, etc.)

Long residence time in combination with high temperatures should be avoided e.g. by pump out material at regular intervals.
During extended interruptions, the barrel temperature should be lowered to about 250-280°C.

It has been found out that heating to the requested processing temperature and shutting down or lowering the temperature is best carried out in two steps.
First, the barrel temperatures are set at the lower processing temperature range for the particular thermoplastic (340 - 350 °C). As soon as these temperatures have reached a steady state, the material in the barrel is pumped out. Second, the barrel temperature can be set to the required processing temperature or the heaters can be shut down.
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com