Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAKEEP® 4000 FP - PEEK - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAKEEP® 4000 FP:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vestakeep datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Texto del producto
Unreinforced, high-viscosity polyether ether ketone fine powder

VESTAKEEP® 4000 FP is an unreinforced, highviscosity polyether ether ketone fine powder. It can be used as a basic resin or in blends with different additives for manufacturing compression molding parts.

The semi-crystalline polymer features superior thermal and chemical resistance. VESTAKEEP® 4000 FP is of low flammability.

VESTAKEEP® 4000 FP is supplied as powder in boxes with moisture-proof polyethyleneliners.

Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at temperatures not exceeding 30°C.

Pigmentation may affect values.

For guidance processing of VESTAKEEP® 4000 FP please follow the general recommendations in our brochure  “VESTAKEEP® High Performance in Powder Form Polyether Ether Ketone Powders“.

The values presented are typical or average values, they do not constitute a specification. 

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM  OR VISIT OUR PRODUCT AT  WWW.INDUSTRIAL.VESTAKEEP.COM
Caracteristicas de procesamiento y fisicasValorUnidadesMétodo de ensayo
ISO Data
Indice de fluidez volumétrico, MVR 11 cm³/10min ISO 1133
Temperatura 380 °C -
Carga 5 kg -
Propiedades mecánicasValorUnidadesMétodo de ensayo
ISO Data
Módulo de tracción 3500 MPa ISO 527
Esfuerzo de fluencia 96 MPa ISO 527
Alarg. en límite elástico 5 % ISO 527
Alarg. nominal a rotura 30 % ISO 527
Resistencia al impacto Charpy, +23°C N kJ/m² ISO 179/1eU
Resistencia al impacto Charpy, -30°C N kJ/m² ISO 179/1eU
Resistencia al impacto Charpy c/entalla, +23°C 7 kJ/m² ISO 179/1eA
Type of failure C - -
Resistencia al impacto Charpy c/entalla, -30°C 6 kJ/m² ISO 179/1eA
Type of failure C - -
Propiedades térmicasValorUnidadesMétodo de ensayo
ISO Data
Temperatura de fusión, 10°C/min 340 °C ISO 11357-1/-3
Estabilidad al calor, 1.80 MPa 150 °C ISO 75-1/-2
Estabilidad al calor, 0.45 MPa 205 °C ISO 75-1/-2
Temp. reblandecimiento Vicat, B 305 °C ISO 306
Otras propiedadesValorUnidadesMétodo de ensayo
Densidad 1300 kg/m³ ISO 1183
Características
Procesamiento y forma de entrega
Transfer Molding, Moldeo por compresión
Forma de suministro
Polvo
Características
Resina de mezcla
Resistencia quimica
Resistencia química general
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com