Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAMID® X7293 - PA12-I - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAMID® X7293:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vestamid datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Texto del producto
High viscosity, plasticized, impact modified, heat- and light-stabilized polyamide 12 compound

VESTAMID® X7293 NC is a plasticized polyamide 12 compound with heat and light stabilizer for the extrusion of flexible tubing and hose,  especially for automotive applications  according to DIN 73378, (PA 12-HIPHL, Type 1), ISO/DIN 7628-1 (PA 12-HIPEHL, Type 1) and SAE J844.
 
VESTAMID® X7293 NC is distinguished by an easy processing as well as by a high impact strength at low temperatures.
 
Properties of compounds based on PA 12 vary little with changing humidity due to low moisture absorption. Parts made of this semi-crystalline material are characterized by exceptional impact strength, low coefficient of friction and good chemical resistance.

VESTAMID® X7293 NC is supplied as cylindrical granules, ready for processing, in moisture-proof bags.

The use of colorants may affect property values. 

Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at temperatures not exceeding 30°C.
 

The results shown have been generated from a low number of production lots. Therefore, they are preliminary and not yet the result of a statistical evaluation. Therefore they must not be used to establish specifications.

For information about processing of VESTAMID®, please follow the general commendations about “Processing of VESTAMID® compounds”. 

The values presented are typical or average values, they do not constitute a specification.

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM OR VISIT OUR PRODUCT AT  WWW.VESTAMID.COM 

 

Caracteristicas de procesamiento y fisicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Indice de fluidez volumétrico, MVR 26 / * cm³/10min ISO 1133
Temperatura 220 / * °C -
Carga 10 / * kg -
Contracción posterior al moldeo, paralelo 0.7 / * % ISO 294-4, 2577
Contracción posterior al moldeo, normal 1.4 / * % ISO 294-4, 2577
Propiedades mecánicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Módulo de tracción 390 / - MPa ISO 527
Esfuerzo de fluencia 25 / - MPa ISO 527
Alarg. en límite elástico 36 / - % ISO 527
Alarg. nominal a rotura >50 / - % ISO 527
Resistencia al impacto Charpy, +23°C N / - kJ/m² ISO 179/1eU
Resistencia al impacto Charpy, -30°C N / - kJ/m² ISO 179/1eU
Resistencia al impacto Charpy c/entalla, +23°C 130 / - kJ/m² ISO 179/1eA
Resistencia al impacto Charpy c/entalla, -30°C 7 / - kJ/m² ISO 179/1eA
Type of failure C / - - -
Propiedades térmicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Temperatura de fusión, 10°C/min 172 / * °C ISO 11357-1/-3
Temp. de transición vítrea, 10°C/min 8 / * °C ISO 11357-1/-2
Estabilidad al calor, 1.80 MPa 45 / * °C ISO 75-1/-2
Estabilidad al calor, 0.45 MPa 100 / * °C ISO 75-1/-2
Temp. reblandecimiento Vicat, B 130 / * °C ISO 306
Coef.de expansión térmica lineal, paralelo 180 / * E-6/K ISO 11359-1/-2
Coef.de expansión térmica lineal, normal 180 / * E-6/K ISO 11359-1/-2
Combustibilidad a 1.5mm esp. nom. HB / * class IEC 60695-11-10
Espesores de probeta 1.6 / * mm -
Propiedades eléctricasSeco / CondUnidadesMétodo de ensayo
ISO Data
Constante dieléctrica, 100Hz 11 / - - IEC 62631-2-1
Constante dieléctrica, 1MHz 4.6 / - - IEC 62631-2-1
Factor de pérdidas dieléctricas, 100Hz 2000 / - E-4 IEC 62631-2-1
Factor de pérdidas dieléctricas, 1MHz 1900 / - E-4 IEC 62631-2-1
Resistividad volumétrica específica 1E10 / - Ohm*m IEC 62631-3-1
Indice comparativo de linea de fuga 600 / - - IEC 60112
Otras propiedadesSeco / CondUnidadesMétodo de ensayo
Absorción de humedad 0.7 / * % Sim. to ISO 62
Densidad 1020 / - kg/m³ ISO 1183
Condiciones de transformaciónValorUnidadesMétodo de ensayo
ISO Data
Moldeo por inyección, temperatura de la masa 220 °C ISO 294
Moldeo por inyección, temperatura del molde 60 °C ISO 294
Moldeo por inyección, velocidad de inyección 200 mm/s ISO 294
Moldeo por inyección, presión de mantenimiento 70 MPa ISO 294
Características
Procesamiento y forma de entrega
Moldeo por inyección, Extrusión de tubería, Extrusión de perfiles, Otros tipos de extrusión
Forma de suministro
Sémola, Color natural
Aditivos
Lubricante, Plastificante
Características especiales
Alto impacto o modificado al impacto, Estable a la luz, Estable contra el calor
Características
Grado tribológico
Resistencia quimica
Resistencia química general
Applicaciones
Automotriz
Disponibilidad regional
Norteamérica, Europa, Asia Pacifico, América del Sur y Centroaméric, Próximo Oriente/Africa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com