Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTODUR® X9400 - PBT-GF10 - Evonik Operations GmbH

Material Data Center offers the following functions for VESTODUR® X9400:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vestodur datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Texto del producto
Glass fiber-reinforced, modified polybutylene terephthalate compound with decreased shrinkage

VESTODUR® X9400 NC is a 10% glass fiber-reinforced, polymer-modified polybutylene terephthalate compound. Moldings of this compound show decreased shrinkage.

 

The compound is suitable for parts that are subjected to high mechanical or thermal loads. Compared with commonly used glass fiber-reinforced PBT compounds with similar stiffness parts of VESTODUR® X9400 have in particular a high surface quality.

 

VESTODUR® X9400 is supplied as cylindrical pellets in polyethylene packaging. 

For information, please follow the general recommendations in our flyer "VESTODUR® Polybutylene terephthalate - Compounds".

 

Pigmentation may affect values.

Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at tempIeratures not exceeding 30°C.
 

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM 
OR VISIT OUR PRODUCT AT  WWW.VESTODUR.COM

Caracteristicas de procesamiento y fisicasValorUnidadesMétodo de ensayo
ISO Data
Contracción posterior al moldeo, paralelo 0.3 % ISO 294-4, 2577
Contracción posterior al moldeo, normal 0.4 % ISO 294-4, 2577
Propiedades mecánicasValorUnidadesMétodo de ensayo
ISO Data
Módulo de tracción 4500 MPa ISO 527
Esfuerzo de fluencia 103 MPa ISO 527
Alarg. en límite elástico 4 % ISO 527
Alarg. nominal a rotura 4 % ISO 527
Resistencia al impacto Charpy, +23°C 50 kJ/m² ISO 179/1eU
Type of failure C - -
Resistencia al impacto Charpy, -30°C 45 kJ/m² ISO 179/1eU
Type of failure C - -
Resistencia al impacto Charpy c/entalla, +23°C 5 kJ/m² ISO 179/1eA
Type of failure C - -
Resistencia al impacto Charpy c/entalla, -30°C 5 kJ/m² ISO 179/1eA
Type of failure C - -
Propiedades térmicasValorUnidadesMétodo de ensayo
ISO Data
Temperatura de fusión, 10°C/min 218 °C ISO 11357-1/-3
Temp. de transición vítrea, 10°C/min 66 °C ISO 11357-1/-2
Estabilidad al calor, 1.80 MPa 110 °C ISO 75-1/-2
Estabilidad al calor, 0.45 MPa 200 °C ISO 75-1/-2
Temp. reblandecimiento Vicat, B 179 °C ISO 306
Coef.de expansión térmica lineal, paralelo 30 E-6/K ISO 11359-1/-2
Coef.de expansión térmica lineal, normal 40 E-6/K ISO 11359-1/-2
Combustibilidad a 1.5mm esp. nom. HB class IEC 60695-11-10
Espesores de probeta 1.6 mm -
Otras propiedadesValorUnidadesMétodo de ensayo
Densidad 1350 kg/m³ ISO 1183
Características
Procesamiento y forma de entrega
Moldeo por inyección
Forma de suministro
Sémola, Color natural
Características especiales
Estable contra el calor
Disponibilidad regional
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.