Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Cadence™ GS2 - Copolyester - Eastman Chemical Co.

Material Data Center offers the following functions for Cadence™ GS2:
unit conversion, PDF datasheet print, comparison with other plastics

Check here, which other Cadence datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Texto del producto

Eastman Cadence™ GS2 is a high-clarity amorphous copolyester for film calendering. Calendered films made of

Eastman Cadence™ copolyesters are non-crystallizing, are halogen-free, offer wide calendering and

thermoforming windows and have good low-temperature toughness. They are cooperative in secondary operations

such as solvent-bonding, lamination, decoration, cold-forming, punching/cutting and embossment.

Propiedades térmicasValorUnidadesMétodo de ensayo
ASTM Data
Coeficiente de dilatación térmica, long. 76.8 E-6/K ASTM D 696
Estabilidad al calor @ 66 psi 71 °C ASTM D 648
Estabilidad al calor @ 264 psi 64 °C ASTM D 648
Temperatura de transición vítrea 82 °C ASTM E 1356
Temperatura Vicat 81 °C ASTM D 1525
Índice de oxigeno límite 24.1 % ASTM D 2863
Propiedades eléctricasValorUnidadesMétodo de ensayo
ASTM Data
Resistencia dieléctrica, tiempo corto 15.6 kV/mm ASTM D 149
Factor de pérdidas dieléctricas, 1 MHz 0.02 - ASTM D 150
Constante dieléctrica, 1 MHz 2.62 - ASTM D 150
Resistividad superficial 1.65E16 Ohm ASTM D 257
Resistividad volumétrica 3.32E16 Ohm*cm ASTM D 257
Resistencia al arco 133 s ASTM D 495
Otras propiedadesValorUnidadesMétodo de ensayo
Absorción de agua, 24hr 0.15 % ASTM D 570
Densidad 1280 kg/m³ ASTM D 792
Características
Procesamiento y forma de entrega
Calandrado, Termoconformación
Características especiales
Transparente
Características
Amorfo, Copolímero
Applicaciones
Construcción
Disponibilidad regional
Norteamérica, Europa, Asia Pacifico, América del Sur y Centroaméric, Próximo Oriente/Africa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.