Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Eastar™ DN004 - Copolyester - Eastman Chemical Co.

Material Data Center offers the following functions for Eastar™ DN004:
unit conversion, PDF datasheet print, comparison with other plastics

Check here, which other Eastar datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Texto del producto

Eastar™ copolyesters are brilliantly clear polymers that have excellent impact strength, chemical resistance, dimensional stability, and low shrinkage rates. Eastar™ DN004 copolyesters are the toughest materials for the

cosmetics and personal care packaging applications. It's very shatter resistant and offers excellent chemical resistance. DN004 contains a mold release.

Caracteristicas de procesamiento y fisicasValorUnidadesMétodo de ensayo
ASTM Data
Contracción posterior al moldeo, paralelo 0.0035 mm/mm ASTM D 955
Propiedades mecánicasValorUnidadesMétodo de ensayo
ISO Data
Esfuerzo de fluencia 46 MPa ISO 527
Alarg. en límite elástico 4.4 % ISO 527
Resistencia a la tracción 47 MPa ISO 527
Alargamiento a rotura 230 % ISO 527
Módulo de flexión, 23°C 1800 MPa ISO 178
Resistencia al impacto Izod con entalla, +23°C 125 kJ/m² ISO 180/1A
Resistencia al impacto Izod con entalla 7.4 kJ/m² ISO 180/1A
Temperatura -40 °C -
Perforación - energía, +23°C 14 J ISO 6603-2
ASTM Data
Módulo de tracción 1800 MPa ASTM D 638
Esfuerzo de fluencia a tracción 45 MPa ASTM D 638
Esfuerzo de fractura a tracción 52 MPa ASTM D 638
Alargamiento a la fluencia 5 % ASTM D 638
Alargamiento a la rotura 330 % ASTM D 638
Módulo de flexión 1800 MPa ASTM D 790
Dureza Rockwell 105 - ASTM D 785
Resistencia al impacto Izod con entalla, 1/8 in N J/m ASTM D 256
Resistencia al impacto Izod con entalla, baja temperatura 64.1 J/m ASTM D 256
Temperatura -40 °C -
Resistencia al impacto Izod, 1/8 in N J/m ASTM D 256
Propiedades térmicasValorUnidadesMétodo de ensayo
ISO Data
Estabilidad al calor, 1.80 MPa 65 °C ISO 75-1/-2
Estabilidad al calor, 0.45 MPa 74 °C ISO 75-1/-2
Temp. reblandecimiento Vicat, A 88 °C ISO 306
Temp. reblandecimiento Vicat, B 79 °C ISO 306
Combustibilidad a 1.5mm esp. nom. HB class IEC 60695-11-10
Espesores de probeta 1.6 mm -
Combustibilidad a espesor h HB class IEC 60695-11-10
Espesores de probeta 3.2 mm -
ASTM Data
Combustibilidad UL 94 HB - UL 94
Espesores de probeta 1.6 mm -
Estabilidad al calor @ 66 psi 74 °C ASTM D 648
Estabilidad al calor @ 264 psi 64 °C ASTM D 648
Temperatura Vicat 88 °C ASTM D 1525
Conductividad térmica, estado sólido 0.0274 W/(m K) ASTM C 177
Propiedades eléctricasValorUnidadesMétodo de ensayo
ASTM Data
Resistencia dieléctrica, tiempo corto 16.3 kV/mm ASTM D 149
Factor de pérdidas dieléctricas, 1 MHz 0.013 - ASTM D 150
Constante dieléctrica, 1 MHz 2.8 - ASTM D 150
Resistividad superficial 1E16 Ohm ASTM D 257
Resistividad volumétrica 1E15 Ohm*cm ASTM D 257
Resistencia al arco 138 s ASTM D 495
Propiedades opticasValorUnidadesMétodo de ensayo
ASTM Data
Opacidad 1 % ASTM D 1003
Transmitancia luminosa 89 % ASTM D 1003
Otras propiedadesValorUnidadesMétodo de ensayo
Densidad 1230 kg/m³ ISO 1183
Absorción de agua, 24hr 0.13 % ASTM D 570
Densidad 1230 kg/m³ ASTM D 792
Recomendación para procesamiento Moldeo por inyecciónValorUnidadesMétodo de ensayo
Temperatura de pre-secado 71 °C -
Tiempo de pre-secado 6 h -
Temperatura de la masa 250 - 270 °C -
Temperatura del molde 15 - 40 °C -
Características
Procesamiento y forma de entrega
Moldeo por inyección
Forma de suministro
Color natural
Aditivos
Desmoldeante
Características especiales
Alto impacto o modificado al impacto
Características
Estabilidad de color, Copolímero
Resistencia quimica
Resistencia química general, Resistencia a solventes, Resistencia a la radiacion
Certifications
Contacto con alimentos
Applicaciones
Médico, Empacado, Equipos deportivos
Disponibilidad regional
Norteamérica, Europa, Asia Pacifico, América del Sur y Centroaméric, Próximo Oriente/Africa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.