Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of LUPOY HR5007AX - (PC+ABS) - LG Chem

Material Data Center offers the following functions for LUPOY HR5007AX:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Lupoy datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Caracteristicas de procesamiento y fisicasValorUnidadesMétodo de ensayo
ISO Data
Índice de fluidez, MFI 15 g/10min ISO 1133
Temperatura 260 °C -
Carga 5 kg -
Contracción posterior al moldeo, paralelo 0 % ISO 294-4, 2577
Contracción posterior al moldeo, normal 0 % ISO 294-4, 2577
ASTM Data
Índice de fluidez, MFI 2.6 g/10min ASTM D 1238
Temperatura 250 °C -
Carga 2.16 kg -
Contracción posterior al moldeo, paralelo 0.0065 mm/mm ASTM D 955
Contracción posterior al moldeo, normal 0.0075 mm/mm ASTM D 955
Propiedades mecánicasValorUnidadesMétodo de ensayo
ISO Data
Módulo de tracción 2040 MPa ISO 527
Esfuerzo de fluencia 50 MPa ISO 527
Alarg. en límite elástico 5.4 % ISO 527
Resistencia a la tracción 48 MPa ISO 527
Alargamiento a rotura 100 % ISO 527
Módulo de flexión, 23°C 2070 MPa ISO 178
Resistencia a la flexión 78 MPa ISO 178
Resistencia al impacto Charpy c/entalla, +23°C 52[1] kJ/m² ISO 179/1eA
Resistencia al impacto Charpy c/entalla, -30°C 27[1] kJ/m² ISO 179/1eA
Resistencia al impacto Izod con entalla, +23°C 50[1] kJ/m² ISO 180/1A
Resistencia al impacto Izod con entalla 23[1] kJ/m² ISO 180/1A
Temperatura -40 °C -
Dureza Rockwell R 112 - ISO 2039-2
ASTM Data
Módulo de tracción 1978 MPa ASTM D 638
Esfuerzo de fluencia a tracción 53 MPa ASTM D 638
Esfuerzo de fractura a tracción 53 MPa ASTM D 638
Alargamiento a la fluencia 5.3 % ASTM D 638
Alargamiento a la rotura 110 % ASTM D 638
Módulo de flexión 2109 MPa ASTM D 790
Resistencia a la flexión 81.4 MPa ASTM D 790
Dureza Rockwell R 112 - ASTM D 785
Resistencia al impacto Izod con entalla, 1/8 in 618 J/m ASTM D 256
Resistencia al impacto Izod con entalla, 1/4 in 471 J/m ASTM D 256
Resistencia al impacto Izod con entalla, baja temperatura 402 J/m ASTM D 256
Temperatura -30 °C -
1: 4 mm
Propiedades térmicasValorUnidadesMétodo de ensayo
ISO Data
Estabilidad al calor, 1.80 MPa 105[2] °C ISO 75-1/-2
Estabilidad al calor, 0.45 MPa 127[2] °C ISO 75-1/-2
Temp. reblandecimiento Vicat, B 124 °C ISO 306
Coef.de expansión térmica lineal, paralelo 77 E-6/K ISO 11359-1/-2
Coef.de expansión térmica lineal, normal 92 E-6/K ISO 11359-1/-2
Combustibilidad a espesor h HB class IEC 60695-11-10
Espesores de probeta 0.8 mm -
ASTM Data
Combustibilidad UL 94 HB - UL 94
Espesores de probeta 0.76 mm -
Coeficiente de dilatación térmica, long. 77 E-6/K ASTM D 696
Coeficiente de dilatación térmica, normal 92 E-6/K ASTM D 696
Estabilidad al calor @ 66 psi 133[3] °C ASTM D 648
Estabilidad al calor @ 264 psi 116[3] °C ASTM D 648
Temperatura Vicat 130 °C ASTM D 1525
2: 4 mm  3: 6.4 mm
Propiedades eléctricasValorUnidadesMétodo de ensayo
ISO Data
Resistividad volumétrica específica 1E15 Ohm*m IEC 62631-3-1
Resistividad superficial específica 1E15 Ohm IEC 62631-3-2
Indice comparativo de linea de fuga 600 - IEC 60112
ASTM Data
Resistencia dieléctrica, tiempo corto 21 kV/mm ASTM D 149
Resistividad superficial 1E15 Ohm ASTM D 257
Resistividad volumétrica 1E17 Ohm*cm ASTM D 257
Otras propiedadesValorUnidadesMétodo de ensayo
Absorción de humedad 0.2 % Sim. to ISO 62
Densidad 1140 kg/m³ ISO 1183
Densidad 1140 kg/m³ ASTM D 792
Recomendación para procesamiento Moldeo por inyecciónValorUnidadesMétodo de ensayo
Temperatura de pre-secado 80 - 100 °C -
Tiempo de pre-secado 4 - 6 h -
Humedad de procesamiento ≤0.02 % -
Temperatura de la masa 250 - 275 °C -
Temperatura del molde 50 - 70 °C -
Zona 1 240 - 270 °C -
Zona 2 245 - 275 °C -
Zona 3 245 - 285 °C -
Temperatura de boquilla 245 - 275 °C -
Características
Procesamiento y forma de entrega
Moldeo por inyección
Características especiales
Estable contra el calor
Applicaciones
Electrica, Uso general
Disponibilidad regional
Norteamérica, Europa, Asia Pacifico, América del Sur y Centroaméric
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.