Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAMID® Care ML16 - PA12 - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAMID® Care ML16:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vestamid datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Texto del producto
Low viscosity polyamide 12 for medical application

VESTAMID® Care ML16 is resistant to body fluids and toxicologically safe.
 

Typical application areas for filled VESTAMID Care ML grades include  catheters, housing parts, monitoring and imaging devices and durable medical equipment.

Advantages at a glance

- High impact resistance

- Easy processability & colorability

- Low sliding friction

- High toughness

- High abrasion resistance

- Density 1.0 g/cc

- High dimensional stability

- High chemical resistance

- Gamma and EtO sterilizable


Biocompatibility of VESTAMID® Care ML
VESTAMID® Care ML grades were tested on biocompatibility for applications within the body of up to 30 days contact time and comply with USP <88> class VI and ISO 10993 standards.

Biocompatibility tests for VESTAMID® Care:
Standard Description
ASTM F756-08 Hemocompatibility
ISO 10993-5 Cytotoxicity
ISO 10993-10 Sensitization: Maximization test according to Magnusson and Kligman
ISO 10993-10 Irritation: Intracutaneous Reactivity
ISO 10993-11 Acute Systemic Toxicity
USP Class VI Acute Systemic Toxicity Intracutaneous Reactivity Muscle Implantation
Processing of VESTAMID® Care
For information about processing of VESTAMID®, please follow the general commendations about “Processing of VESTAMID® compounds”. 
 
FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM
OR VISIT OUR PRODUCT AT  WWW.EVONIK.COM/MEDICAL-TECHNOLOGY
Caracteristicas de procesamiento y fisicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Indice de fluidez volumétrico, MVR 46 / * cm³/10min ISO 1133
Temperatura 210 / * °C -
Carga 2.16 / * kg -
Contracción posterior al moldeo, paralelo 0.9 / * % ISO 294-4, 2577
Contracción posterior al moldeo, normal 1.1 / * % ISO 294-4, 2577
Propiedades mecánicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Módulo de tracción 1400 / - MPa ISO 527
Esfuerzo de fluencia 43 / - MPa ISO 527
Alarg. en límite elástico 5 / - % ISO 527
Alarg. nominal a rotura >50 / - % ISO 527
Resistencia al impacto Charpy, +23°C N / - kJ/m² ISO 179/1eU
Resistencia al impacto Charpy, -30°C N / - kJ/m² ISO 179/1eU
Resistencia al impacto Charpy c/entalla, +23°C 4 / - kJ/m² ISO 179/1eA
Type of failure C / - - -
Resistencia al impacto Charpy c/entalla, -30°C 5 / - kJ/m² ISO 179/1eA
Type of failure C / - - -
Dureza Shore D 75 / * - ISO 7619-1
Propiedades térmicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Temperatura de fusión, 10°C/min 178 / * °C ISO 11357-1/-3
Temp. de transición vítrea, 10°C/min 45 / * °C ISO 11357-1/-2
Estabilidad al calor, 1.80 MPa 50 / * °C ISO 75-1/-2
Estabilidad al calor, 0.45 MPa 110 / * °C ISO 75-1/-2
Temp. reblandecimiento Vicat, B 140 / * °C ISO 306
Coef.de expansión térmica lineal, paralelo 150 / * E-6/K ISO 11359-1/-2
Combustibilidad a 1.5mm esp. nom. HB / * class IEC 60695-11-10
Espesores de probeta 1.6 / * mm -
Propiedades eléctricasSeco / CondUnidadesMétodo de ensayo
ISO Data
Constante dieléctrica, 100Hz 3.1 / - - IEC 62631-2-1
Constante dieléctrica, 1MHz 2.9 / - - IEC 62631-2-1
Factor de pérdidas dieléctricas, 100Hz 400 / - E-4 IEC 62631-2-1
Factor de pérdidas dieléctricas, 1MHz 300 / - E-4 IEC 62631-2-1
Resistividad volumétrica específica 1E11 / - Ohm*m IEC 62631-3-1
Otras propiedadesSeco / CondUnidadesMétodo de ensayo
Absorción de agua 1.5 / * % Sim. to ISO 62
Absorción de humedad 0.7 / * % Sim. to ISO 62
Densidad 1020 / - kg/m³ ISO 1183
Características
Procesamiento y forma de entrega
Moldeo por inyección
Forma de suministro
Sémola
Características especiales
Alto impacto o modificado al impacto, Esterilizable, Esterilización por óxido de etileno (EtO), Gamma irradiation sterilization
Características
Grado tribológico
Resistencia quimica
Resistencia química general
Certifications
Grado médico, Biocompatibility ISO 10993, USP Class VI
Applicaciones
Médico
Disponibilidad regional
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com