Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of CELANEX® 3126 - PBT-GF10 - Celanese

Material Data Center offers the following functions for CELANEX® 3126:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Celanex datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Informations produit
Celanex 3126 is a non-exuding flame retarded, 10% fiberglass reinforced polybutylene terephthalate which has an excellent balance of mechanical properties and processability. It is well suited for electrical connector applications where its UL approved 50% regrind use capability allows maximum use of purchased product.

Flammability @1.6mm nom. thickn.V-0-
Flammability at thickness h (0.38 mm)V-0UL recognition (h)
Caractéristiques des transformations/physiquesValeurUnitéNorme du test
ISO Data
Indice de fluidité à chaud en volume, MVR 15 cm³/10min ISO 1133
Température 250 °C -
Charge 2.16 kg -
Retrait au moulage, parallèle 1.1 % ISO 294-4, 2577
Retrait au moulage, perpendiculaire 1.1 % ISO 294-4, 2577
Propriétés mécaniquesValeurUnitéNorme du test
ISO Data
Module en traction 5200 MPa ISO 527
Contrainte à la rupture 85 MPa ISO 527
Déformation à la rupture 3 % ISO 527
Résistance au choc Charpy, +23°C 24 kJ/m² ISO 179/1eU
Résistance au choc Charpy, -30°C 24 kJ/m² ISO 179/1eU
Résistance au choc Charpy (entaillé), +23°C 5 kJ/m² ISO 179/1eA
Résistance au choc Charpy (entaillé), -30°C 5 kJ/m² ISO 179/1eA
Propriétés thermiquesValeurUnitéNorme du test
ISO Data
Température de fusion, 10°C/min 225 °C ISO 11357-1/-3
Température de transition vitreuse, 10°C/min 60 °C ISO 11357-1/-2
Température de fléchissement s/chrg, 1.80 MPa 195 °C ISO 75-1/-2
Température de fléchissement s/chrg, 8.00 MPa 56 °C ISO 75-1/-2
Température de ramolliss. Vicat, B 205 °C ISO 306
Coeffic. de dilatation therm. linéique, parallèle 60 E-6/K ISO 11359-1/-2
Inflammabilité ep. nom. 1.5 mm V-0 class IEC 60695-11-10
Epaisseur de l'éprouvette 1.5 mm -
Inflammabilité pr. épaisseur h V-0 class IEC 60695-11-10
Epaisseur de l'éprouvette 0.4 mm -
Yellow Card disponible oui - -
Aptitude à l'allumage 30 % ISO 4589-1/-2
Propriétés électriquesValeurUnitéNorme du test
ISO Data
Permittivité relative, 100Hz 3.6 - IEC 62631-2-1
Permittivité relative, 1MHz 3.5 - IEC 62631-2-1
Facteur de pertes, 100Hz 33 E-4 IEC 62631-2-1
Facteur de pertes, 1MHz 165 E-4 IEC 62631-2-1
Résistivité transversale >1E13 Ohm*m IEC 62631-3-1
Résistivité superficielle >1E15 Ohm IEC 62631-3-2
Rigidité diélectrique 29 kV/mm IEC 60243-1
Propriétés diversesValeurUnitéNorme du test
Absorption d'eau 0.45 % Sim. to ISO 62
Absorption d'humidité 0.2 % Sim. to ISO 62
Masse volumique 1530 kg/m³ ISO 1183
Recommandations pour la transformation Moulage par injectionValeurUnitéNorme du test
Pré-séchage - température 120 - 140 °C -
Pré-séchage - temps 2 - 4 h -
L'humidité de traitement ≤0.02 % -
Température de la matière fondue 260 - 270 °C -
Température du moule 75 - 85 °C -
Fonctions
Volume spécifique (pvT) , CELANEX® 3126, PBT-GF10, Celanese
Caractéristiques
Transformation
Moulage par injection
Conditionnement
Granulés
Additifs
Agent de démoulage
Propriétés spéciales
Ignifugé, Stabilisé à la chaleur
Applications
Électrotechnique et électrique
Disponibilité régionale
Europe
Autres informations
Moulages par injection
To avoid hydrolytic degradation during processing, CELANEX resins have to be dried to a moisture level equal to or less than 0,02%. The drying should be done in a dry-air dryer (dew point < -30°C) with a temperature of 120 to 140 °C and a drying time of 2 to 4 hours. In case of longer residence times in the dry-air dryer, the temperature should be reduced to 100°C.
The time between drying and processing should be kept as short as possible. The processing machine feed hopper should be closed during the processing operation.
Melt Temperature 260-270 °C
Mold Temperature *) 75-85 °C
Maximum Barrel Residence Time **) 5-10 min
Injection Speed fast
Peripheral screw speed max.0,3 m/sec
Back Pressure 10-30 bar
Injection Pressure 600-1000 bar
Holding Pressure 400-800 bar
Nozzle Design open design preferred

Injection speed, injection pressure and holding pressure have to be optimized to the individual article geometry. To avoid material degradation during processing low back pressure and minimum screw speed have to be used. Overheating of the material has to be avoided. For grades containing flame retardants, a maximum temperature of 265 °C should not be exceeded.

Celanese recommends only externally heated hot runner systems.

*) For moulded parts with especially high requirements to the surface quality or dimensional stability, a mold temperature of up to 110 °C can be advantageous.

**) If the cylinder temperatures are higher than the recommended maximum temperatures, the max. residence time in the barrel has to be reduced.
Conditions générales
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com