Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Eastar™ EN001 - Copolyester - Eastman Chemical Co.

Material Data Center offers the following functions for Eastar™ EN001:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Eastar datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Informations produit

Eastar™ EN001 Copolyester is a thermoplastic polyester copolymer and is suitable for food packaging applications.

Eastar™ EN001 Copolyester has a relatively slow crystallization rate. This broadens the operating window for extrusion and forming processes and helps maintain good clarity when processing much thicker sheet. Eastar™ EN001 copolyester can also be used for injection molding applications. It is the preferred general-purpose crystallizable PET for thermoforming.

Eastar™ EN001 copolyester is regulated for use in food packaging applications in accordance with US FDA Regulation 21 CFR 177.1315. It is lawful for use under US Department of Agriculture Food Safety Inspection Service regulations as a packaging material for meat or poultry food products prepared under federal inspection.




Propriétés mécaniquesValeurUnitéNorme du test
ISO Data
Module en traction 2400 MPa ISO 527
Contrainte d'écoulement 57 MPa ISO 527
Contrainte à la rupture 25 MPa ISO 527
Déformation à la rupture 120 % ISO 527
Module de flexion, 23°C 2300 MPa ISO 178
Résistance au choc Izod, +23°C N kJ/m² ISO 180/1U
Résistance au choc Izod avec entaille, +23°C 4.5 kJ/m² ISO 180/1A
Résistance au choc Izod avec entaille 3.1 kJ/m² ISO 180/1A
Température -40 °C -
Perforation - Energie, +23°C 15 J ISO 6603-2
Dureté Rockwell R 114 - ISO 2039-2
ASTM Data
Module en traction 2400 MPa ASTM D 638
Module de traction d’élasticité 58 MPa ASTM D 638
Résistance de traction à la rupture 25 MPa ASTM D 638
Allongement à la rupture 120 % ASTM D 638
Module de flexion 2500 MPa ASTM D 790
Dureté Rockwell 112 - ASTM D 785
Izod choc avec entaille, 1/8 in 40 J/m ASTM D 256
Izod choc avec entaille, bas température 27 J/m ASTM D 256
Température -40 °C -
Résistance au choc Izod, 1/8 in N J/m ASTM D 256
Propriétés thermiquesValeurUnitéNorme du test
ISO Data
Température de fléchissement s/chrg, 1.80 MPa 65 °C ISO 75-1/-2
Température de fléchissement s/chrg, 0.45 MPa 69 °C ISO 75-1/-2
ASTM Data
DTUL à 66 psi 68.9 °C ASTM D 648
DTUL à 264 psi 65 °C ASTM D 648
Propriétés optiquesValeurUnitéNorme du test
ASTM Data
Haze 1 % ASTM D 1003
Lumière á Transmittance 84 % ASTM D 1003
Propriétés diversesValeurUnitéNorme du test
Masse volumique 1330 kg/m³ ISO 1183
Densité 1330 kg/m³ ASTM D 792
Caractéristiques
Transformation
Moulage par injection, Extrusion (autres), Thermoformage
Caractéristiques
Copolymère
Certifications
Contact alimentaire, FDA 21 CFR approbation
Applications
Automobile, Emballage, Sport
Disponibilité régionale
Amérique du nord, Europe, Asia Pacific, South and Central America, Proche-Orient/Afrique
Conditions générales
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com