Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Makrolon® 2858 RE - PC - Covestro Deutschland AG

Material Data Center offers the following functions for Makrolon® 2858 RE:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Makrolon datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Informations produit
  • MVR (300 °C/1.2 kg) 9.0 cm³/10 min
  • medical devices
  • suitable for ETO and steam sterilization at 121 °C
  • biocompatible according to many ISO 10993-1 test requirements
  • medium viscosity
  • easy release
Caractéristiques des transformations/physiquesValeurUnitéNorme du test
ISO Data
Indice de fluidité à chaud en volume, MVR 9 cm³/10min ISO 1133
Température 300 °C -
Charge 1.2 kg -
Indice de fluidité, MFI 10 g/10min ISO 1133
Température 300 °C -
Charge 1.2 kg -
Retrait au moulage, parallèle 0.7 % ISO 294-4, 2577
Retrait au moulage, perpendiculaire 0.8 % ISO 294-4, 2577
Propriétés mécaniquesValeurUnitéNorme du test
ISO Data
Module en traction 2400 MPa ISO 527
Contrainte d'écoulement 66 MPa ISO 527
Déformation au seuil d'écoulement 6.1 % ISO 527
Déformation nominale à la rupture >50 % ISO 527
Module de flexion, 23°C 2400 MPa ISO 178
Résistance à la flexion 97 MPa ISO 178
Module de fluage en traction, 1h 2200 MPa ISO 899-1
Module de fluage en traction, 1000h 1900 MPa ISO 899-1
Résistance au choc Charpy, +23°C N kJ/m² ISO 179/1eU
Résistance au choc Charpy (entaillé), +23°C 75 kJ/m² ISO 179/1eA
Type de défaillance P - -
Résistance au choc Charpy (entaillé), -30°C 16 kJ/m² ISO 179/1eA
Type de défaillance C - -
Résistance au choc Izod avec entaille, +23°C 70 kJ/m² ISO 180/1A
Résistance au choc Izod avec entaille 15 kJ/m² ISO 180/1A
Température -30 °C -
Perforation - force maximum, +23°C 5400 N ISO 6603-2
Perforation - force maximum, -30°C 6300 N ISO 6603-2
Perforation - Energie, +23°C 60 J ISO 6603-2
Perforation - Energie, -30°C 65 J ISO 6603-2
Ball indentation hardness 115 MPa ISO 2039-1
Propriétés thermiquesValeurUnitéNorme du test
ISO Data
Température de transition vitreuse, 10°C/min 145 °C ISO 11357-1/-2
Température de fléchissement s/chrg, 1.80 MPa 125 °C ISO 75-1/-2
Température de fléchissement s/chrg, 0.45 MPa 137 °C ISO 75-1/-2
Température de ramolliss. Vicat, B 145 °C ISO 306
Coeffic. de dilatation therm. linéique, parallèle 65 E-6/K ISO 11359-1/-2
Coeffic. de dilatation therm. linéique, perpend. 65 E-6/K ISO 11359-1/-2
Inflammabilité pr. épaisseur h V-2 class IEC 60695-11-10
Epaisseur de l'éprouvette 0.8 mm -
Yellow Card disponible oui - -
Aptitude à l'allumage 28 % ISO 4589-1/-2
Glow Wire Flammability Index (GWFI) 850 °C IEC 60695-2-12
GWFI - thickness tested (1) 1.5 mm -
Glow Wire Flammability Index (GWFI) 930 °C IEC 60695-2-12
GWFI - thickness tested (2) 3 mm -
Glow Wire Ignition Temperature (GWIT) 875 °C IEC 60695-2-13
GWIT - thickness tested (1) 0.75 mm -
Glow Wire Ignition Temperature (GWIT) 875 °C IEC 60695-2-13
GWIT - thickness tested (2) 1.5 mm -
Glow Wire Ignition Temperature (GWIT) 900 °C IEC 60695-2-13
GWIT - thickness tested (3) 3 mm -
Other Standards[S]
Conductivité thermique, l'état solide 0.2 W/(m K) ISO 8302
S: These properties are reported by the producer according standards that are different to our defaults.
Propriétés électriquesValeurUnitéNorme du test
ISO Data
Permittivité relative, 100Hz 3.1 - IEC 62631-2-1
Permittivité relative, 1MHz 3 - IEC 62631-2-1
Facteur de pertes, 100Hz 5 E-4 IEC 62631-2-1
Facteur de pertes, 1MHz 90 E-4 IEC 62631-2-1
Résistivité transversale >1E13 Ohm*m IEC 62631-3-1
Résistivité superficielle >1E15 Ohm IEC 62631-3-2
Rigidité diélectrique 34 kV/mm IEC 60243-1
Indice de résistance au cheminement 250 - IEC 60112
Propriétés optiquesValeurUnitéNorme du test
ISO Data
Haze 0.8 - ISO 14782
Transmittance 89 % ISO 13468-1, -2
Other Standards[S]
Indice de réfraction 1.59 - ISO 489
S: These properties are reported by the producer according standards that are different to our defaults.
Propriétés diversesValeurUnitéNorme du test
Absorption d'eau 0.3 % Sim. to ISO 62
Absorption d'humidité 0.12 % Sim. to ISO 62
Masse volumique 1200 kg/m³ ISO 1183
Bulk density 660 kg/m³ -
Préparation et conditionnement des éprouvettesValeurUnitéNorme du test
ISO Data
Injection, température de la matière fondue 300 °C ISO 294
Injection, température du moule 80 °C ISO 294
Injection, vitesse d'injection 200 mm/s ISO 294
Recommandations pour la transformation Moulage par injectionValeurUnitéNorme du test
Pré-séchage - température 120 °C -
Pré-séchage - temps 2 - 3 h -
L'humidité de traitement ≤0.02 % -
Température de la matière fondue 280 - 320 °C -
Température du moule 80 - 120 °C -
Zone 1 250 - 260 °C -
Zone 2 270 - 280 °C -
Zone 3 280 - 290 °C -
Température de la buse 290 - 300 °C -
Contre-pression 5 - 15 MPa -
Caractéristiques
Transformation
Moulage par injection
Conditionnement
Granulés
Additifs
Agent de démoulage
Propriétés spéciales
Transparent, Opaque, Stérilisable, Stérilisation par oxyde d'éthylène (EtO), Stérilisation à la vapeur
Certifications
Contient des ressources renouvelables, Résine de contenu recyclé, Grade médical, Biocompatibility ISO 10993, ISCC Plus
Applications
Médical
Disponibilité régionale
Conditions générales
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com