Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of RamOfin PPH300G4NT - PP-GF20 - Polyram

Material Data Center offers the following functions for RamOfin PPH300G4NT:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Ramofin datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Caractéristiques des transformations/physiquesValeurUnitéNorme du test
ISO Data
Indice de fluidité, MFI 6.4 g/10min ISO 1133
Température 230 °C -
Charge 2.16 kg -
Other Standards[S]
Retrait au moulage, parallèle 0.3 % Producer Method
Retrait au moulage, perpendiculaire 0.8 % Producer Method
S: These properties are reported by the producer according standards that are different to our defaults.
Propriétés mécaniquesValeurUnitéNorme du test
ISO Data
Module en traction 4800 MPa ISO 527
Résistance à la traction 78 MPa ISO 527
Déformation à la rupture 3.4 % ISO 527
Module de flexion, 23°C 3800 MPa ISO 178
Résistance à la flexion 125 MPa ISO 178
Résistance au choc Izod avec entaille, +23°C 11 kJ/m² ISO 180/1A
Résistance au choc Izod avec entaille 8.4 kJ/m² ISO 180/1A
Température -30 °C -
Propriétés thermiquesValeurUnitéNorme du test
ISO Data
Température de fléchissement s/chrg, 1.80 MPa 140 °C ISO 75-1/-2
Température de fléchissement s/chrg, 0.45 MPa 155 °C ISO 75-1/-2
Inflammabilité pr. épaisseur h HB class IEC 60695-11-10
Epaisseur de l'éprouvette 3.0 mm -
Vitesse de combustion, FMVSS, épaisseur 1 mm 100 mm/min ISO 3795 (FMVSS 302)
Propriétés diversesValeurUnitéNorme du test
Masse volumique 1030 kg/m³ ISO 1183
Recommandations pour la transformation Moulage par injectionValeurUnitéNorme du test
Pré-séchage - température 80 °C -
Pré-séchage - temps 2 - 4 h -
L'humidité de traitement ≤0.1 % -
Température du moule 30 - 70 °C -
Température - Zone d'alimentation 60 - 70 °C -
Zone 1 200 - 230 °C -
Zone 2 200 - 230 °C -
Zone 3 200 - 250 °C -
Caractéristiques
Transformation
Moulage par injection
Conditionnement
Couleurs naturelles
Caractéristiques
Homopolymère
Certifications
RoHS
Disponibilité régionale
Amérique du nord, Europe, Asia Pacific, South and Central America, Proche-Orient/Afrique
Conditions générales
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com