Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAKEEP® i2 G - PEEK - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAKEEP® i2 G:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vestakeep datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Informations produit
Implantable grade polyether ether ketone resin for permanent implants

VESTAKEEP® i2 G is a natural colored, standard viscosity polyether ether ketone (PEEK) that is especially designed for long term implantable medical devices. This grade is often used for injection molding processing technologies due to its good flowability.

Proven Biocompatibility of VESTAKEEP® i-Grades
The extra high purity and extended quality measures make VESTAKEEP® i-Grade materials an excellent choice for permanent implants.

For VESTAKEEP® i2 G, biocompatibility has been tested following ISO 10993-1 recommendations for permanent tissue/bone contact and USP Class VI.

VESTAKEEP® i2 G complies ASTM F2026 “Standard Specification for Polyetheretherketone (PEEK) Polymers for Surgical Implant Applications”.

A summary of biocompatibility test results is available upon request.

Biocompatibility tests available for i2 G


Processing of VESTAKEEP® i-Grades
VESTAKEEP® i2 G can be processed by common melt processing techniques like injection molding and extrusion.

We recommend a melt temperature between 360°C and 380°C during the injection molding process. The mold temperature should be within a range of 160°C to 200°C, preferably 180°C.

Our technical experts would appreciate to give you support regarding the special requirements for the processing of VESTAKEEP® i2 G.

Delivery of VESTAKEEP® i-Grades
VESTAKEEP® i2 G is supplied as cylindrical pellets in 10 kg boxes with moisture-proof polyethylene liners.

The values presented are typical or average values, they do not constitute a specification. 

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM
OR VISIT OUR PRODUCT AT  WWW.EVONIK.COM/MEDICAL-TECHNOLOGY
Caractéristiques des transformations/physiquesValeurUnitéNorme du test
ISO Data
Indice de fluidité à chaud en volume, MVR 68 cm³/10min ISO 1133
Température 380 °C -
Charge 5 kg -
Retrait au moulage, parallèle 1.1 % ISO 294-4, 2577
Retrait au moulage, perpendiculaire 1.1 % ISO 294-4, 2577
Propriétés mécaniquesValeurUnitéNorme du test
ISO Data
Module en traction 3700 MPa ISO 527
Contrainte d'écoulement 98 MPa ISO 527
Déformation au seuil d'écoulement 5 % ISO 527
Déformation nominale à la rupture 20 % ISO 527
Résistance au choc Charpy, +23°C N kJ/m² ISO 179/1eU
Résistance au choc Charpy, -30°C N kJ/m² ISO 179/1eU
Résistance au choc Charpy (entaillé), +23°C 6 kJ/m² ISO 179/1eA
Type de défaillance C - -
Résistance au choc Charpy (entaillé), -30°C 6 kJ/m² ISO 179/1eA
Type de défaillance C - -
Propriétés thermiquesValeurUnitéNorme du test
ISO Data
Température de fusion, 10°C/min 342 °C ISO 11357-1/-3
Température de transition vitreuse, 10°C/min 150 °C ISO 11357-1/-2
Température de fléchissement s/chrg, 1.80 MPa 150 °C ISO 75-1/-2
Température de fléchissement s/chrg, 0.45 MPa 205 °C ISO 75-1/-2
Température de ramolliss. Vicat, B 310 °C ISO 306
Coeffic. de dilatation therm. linéique, parallèle 60 E-6/K ISO 11359-1/-2
Aptitude à l'allumage 38 % ISO 4589-1/-2
Propriétés électriquesValeurUnitéNorme du test
ISO Data
Permittivité relative, 100Hz 2.8 - IEC 62631-2-1
Permittivité relative, 1MHz 2.8 - IEC 62631-2-1
Facteur de pertes, 1MHz 50 E-4 IEC 62631-2-1
Résistivité transversale >1E13 Ohm*m IEC 62631-3-1
Indice de résistance au cheminement 200 - IEC 60112
Propriétés diversesValeurUnitéNorme du test
Absorption d'eau 0.4 % Sim. to ISO 62
Absorption d'humidité 0.12 % Sim. to ISO 62
Masse volumique 1300 kg/m³ ISO 1183
Préparation et conditionnement des éprouvettesValeurUnitéNorme du test
ISO Data
Injection, température de la matière fondue 380 °C ISO 294
Injection, température du moule 180 °C ISO 294
Injection, vitesse d'injection 200 mm/s ISO 294
Caractéristiques
Transformation
Moulage par injection, Extrusion (autres)
Conditionnement
Granulés, Couleurs naturelles
Certifications
Grade médical, Biocompatibility ISO 10993, USP Class VI approbation
Applications
Médical
Disponibilité régionale
Amérique du nord, Europe, Asia Pacific, South and Central America, Proche-Orient/Afrique
Conditions générales
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com