Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAMID® Care ML-GB30 - PA12-GB30 - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAMID® Care ML-GB30:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Vestamid datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Informations produit

Microglass bead-filled (30%) PA12 resin for the injection moulding of rigid, low-warpage and dimensionally accurate mouldings

 

Biocompatibility of VESTAMID® Care
VESTAMID® Care ML grades were tested on biocompatibility for applications within the body of up to 30 days contact time and comply with USP <88> class VI and ISO 10993 standards.

Biocompatibility tests for VESTAMID® Care:
Standard Description
ASTM F756-08 Hemocompatibility
ISO 10993-5 Cytotoxicity
ISO 10993-10 Sensitization: Maximization test according to Magnusson and Kligman
ISO 10993-10 Irritation: Intracutaneous Reactivity
ISO 10993-11 Acute Systemic Toxicity
USP Class VI Acute Systemic Toxicity Intracutaneous Reactivity Muscle Implantation
 
Processing of VESTAMID® Care
For information about processing of VESTAMID®, please follow the general commendations about “Processing of VESTAMID® compounds”. 



FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM
OR VISIT OUR PRODUCT AT  WWW.EVONIK.COM/MEDICAL-TECHNOLOGY


 

Caractéristiques des transformations/physiquessec / condUnitéNorme du test
ISO Data
Indice de fluidité à chaud en volume, MVR 100 / * cm³/10min ISO 1133
Température 275 / * °C -
Charge 5 / * kg -
Retrait au moulage, parallèle 0.6 / * % ISO 294-4, 2577
Retrait au moulage, perpendiculaire 0.7 / * % ISO 294-4, 2577
Propriétés mécaniquessec / condUnitéNorme du test
ISO Data
Module en traction 2100 / 1800 MPa ISO 527
Contrainte d'écoulement 47 / 37 MPa ISO 527
Déformation au seuil d'écoulement 5 / 5 % ISO 527
Déformation nominale à la rupture 20 / >50 % ISO 527
Module de fluage en traction, 1h * / 1600 MPa ISO 899-1
Module de fluage en traction, 1000h * / 1100 MPa ISO 899-1
Résistance au choc Charpy, +23°C 160 / N kJ/m² ISO 179/1eU
Type de défaillance C / - - -
Résistance au choc Charpy, -30°C 160 / N kJ/m² ISO 179/1eU
Type de défaillance C / - - -
Résistance au choc Charpy (entaillé), +23°C 4.4 / 6 kJ/m² ISO 179/1eA
Type de défaillance C / C - -
Résistance au choc Charpy (entaillé), -30°C 6 / 6 kJ/m² ISO 179/1eA
Type de défaillance C / C - -
Propriétés thermiquessec / condUnitéNorme du test
ISO Data
Température de fusion, 10°C/min 178 / * °C ISO 11357-1/-3
Température de fléchissement s/chrg, 1.80 MPa 55 / * °C ISO 75-1/-2
Température de fléchissement s/chrg, 0.45 MPa 150 / * °C ISO 75-1/-2
Température de ramolliss. Vicat, B 155 / * °C ISO 306
Coeffic. de dilatation therm. linéique, parallèle 130 / * E-6/K ISO 11359-1/-2
Coeffic. de dilatation therm. linéique, perpend. 130 / * E-6/K ISO 11359-1/-2
Inflammabilité ep. nom. 1.5 mm HB / * class IEC 60695-11-10
Epaisseur de l'éprouvette 1.6 / * mm -
Propriétés électriquessec / condUnitéNorme du test
ISO Data
Permittivité relative, 100Hz 4.1 / 5 - IEC 62631-2-1
Permittivité relative, 1MHz 3.5 / 4 - IEC 62631-2-1
Facteur de pertes, 100Hz 310 / 600 E-4 IEC 62631-2-1
Facteur de pertes, 1MHz 230 / 370 E-4 IEC 62631-2-1
Résistivité transversale >1E13 / 2E12 Ohm*m IEC 62631-3-1
Résistivité superficielle * / 1E15 Ohm IEC 62631-3-2
Rigidité diélectrique - / 36 kV/mm IEC 60243-1
Indice de résistance au cheminement 600 / 600 - IEC 60112
Propriétés diversessec / condUnitéNorme du test
Absorption d'eau 1.1 / * % Sim. to ISO 62
Absorption d'humidité 0.5 / * % Sim. to ISO 62
Masse volumique 1250 / 1260 kg/m³ ISO 1183
Fonctions
Viscosité / Vitesse de cisaillement , VESTAMID® Care ML-GB30, PA12-GB30, Evonik
Contrainte de cisaillement / Vit. de cisaillement , VESTAMID® Care ML-GB30, PA12-GB30, Evonik
Module de cisaillement dynamique / Température , VESTAMID® Care ML-GB30 (sec), PA12-GB30, Evonik
Contrainte / Déformation , VESTAMID® Care ML-GB30 (sec), PA12-GB30, Evonik
Module sécant / Déformation , VESTAMID® Care ML-GB30 (sec), PA12-GB30, Evonik
Contrainte / Déformation (isochrone) 23°C, VESTAMID® Care ML-GB30 (cond.), PA12-GB30, Evonik
Module de fluage / Temps 23°C, VESTAMID® Care ML-GB30 (cond.), PA12-GB30, Evonik
Courbe de fluage 23°C, VESTAMID® Care ML-GB30 (cond.), PA12-GB30, Evonik
Caractéristiques
Transformation
Moulage par injection
Conditionnement
Granulés
Caractéristiques
Bas gauchissement
Certifications
Grade médical, Biocompatibility ISO 10993, USP Class VI approbation
Applications
Médical
Disponibilité régionale
Conditions générales
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com