Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAMID® Care ML19 - PA12 - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAMID® Care ML19:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vestamid datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Informations produit
Medium viscosity Polyamide 12 for medical application

VESTAMID® Care ML19 is resistant to body fluids and toxicologically safe.
 

Typical application areas for filled VESTAMID Care ML grades include  catheters, housing parts, monitoring and imaging devices and durable medical equipment.

The advantages at a glance:

  • High flexibility & elasticity
  • Good rebound properties
  • High impact resistance
  • Excellent dimensional stability
  • High chemical resistance
  • Easy processability & colorability
  • Plasticizer-free
  • Gamma and EtO sterilization resistant
  • Tough and resilient

 

Biocompatibility of VESTAMID® Care ML

Biocompatiblity was tested following ISO10993-1 recommendations for a surface medical device with up to 30 days body contact.
 
The material fulfills the requirements of USP<88> class VI.
 
Tests were performed by independent, certified laboratories.

Biocompatibility tests for VESTAMID® Care:
Standard Description
ASTM F756-08 Hemocompatibility
ISO 10993-5 Cytotoxicity
ISO 10993-10 Sensitization: Maximization test according to Magnusson and Kligman
ISO 10993-10 Irritation: Intracutaneous Reactivity
ISO 10993-11 Acute Systemic Toxicity
USP Class VI Acute Systemic Toxicity Intracutaneous Reactivity Muscle Implantation


Processing of VESTAMID® Care
For information about processing of VESTAMID®, please follow the general commendations about “Processing of VESTAMID® compounds”. 

The values presented are typical or average values, they do not constitute a specification. 

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM
OR VISIT OUR PRODUCT AT  WWW.EVONIK.COM/MEDICAL-TECHNOLOGY
Caractéristiques des transformations/physiquessec / condUnitéNorme du test
ISO Data
Indice de fluidité à chaud en volume, MVR 27 / * cm³/10min ISO 1133
Température 240 / * °C -
Charge 5 / * kg -
Retrait au moulage, parallèle 0.8 / * % ISO 294-4, 2577
Retrait au moulage, perpendiculaire 1.1 / * % ISO 294-4, 2577
Propriétés mécaniquessec / condUnitéNorme du test
ISO Data
Module en traction 1400 / 1000 MPa ISO 527
Contrainte d'écoulement 43 / 38 MPa ISO 527
Déformation au seuil d'écoulement 5 / 15 % ISO 527
Déformation nominale à la rupture >50 / >50 % ISO 527
Résistance au choc Charpy, +23°C N / N kJ/m² ISO 179/1eU
Résistance au choc Charpy, -30°C N / N kJ/m² ISO 179/1eU
Résistance au choc Charpy (entaillé), +23°C 7 / 10 kJ/m² ISO 179/1eA
Type de défaillance C / C - -
Résistance au choc Charpy (entaillé), -30°C 7 / 5 kJ/m² ISO 179/1eA
Type de défaillance C / C - -
Dureté Shore D 73 / * - ISO 7619-1
Propriétés thermiquessec / condUnitéNorme du test
ISO Data
Température de fusion, 10°C/min 178 / * °C ISO 11357-1/-3
Température de transition vitreuse, 10°C/min 45 / * °C ISO 11357-1/-2
Température de fléchissement s/chrg, 1.80 MPa 50 / * °C ISO 75-1/-2
Température de fléchissement s/chrg, 0.45 MPa 110 / * °C ISO 75-1/-2
Température de ramolliss. Vicat, B 140 / * °C ISO 306
Coeffic. de dilatation therm. linéique, parallèle 150 / * E-6/K ISO 11359-1/-2
Inflammabilité ep. nom. 1.5 mm HB / * class IEC 60695-11-10
Epaisseur de l'éprouvette 1.6 / * mm -
Propriétés électriquessec / condUnitéNorme du test
ISO Data
Permittivité relative, 100Hz 3.8 / - - IEC 62631-2-1
Permittivité relative, 1MHz 3 / - - IEC 62631-2-1
Facteur de pertes, 100Hz 500 / - E-4 IEC 62631-2-1
Facteur de pertes, 1MHz 323 / - E-4 IEC 62631-2-1
Résistivité transversale >1E13 / 2.2E12 Ohm*m IEC 62631-3-1
Propriétés diversessec / condUnitéNorme du test
Absorption d'eau 1.5 / * % Sim. to ISO 62
Absorption d'humidité 0.7 / * % Sim. to ISO 62
Masse volumique 1020 / - kg/m³ ISO 1183
Préparation et conditionnement des éprouvettesValeurUnitéNorme du test
ISO Data
Injection, température de la matière fondue 220 °C ISO 294
Injection, température du moule 60 °C ISO 294
Injection, vitesse d'injection 200 mm/s ISO 294
Caractéristiques
Transformation
Moulage par injection
Conditionnement
Granulés
Propriétés spéciales
Modifié choc, Stérilisable, Stérilisation par oxyde d'éthylène (EtO), Stérilisation par rayonnement gamma
Caractéristiques
Grade tribologique
Résistance Chimique
Résistance chimique générale
Certifications
Grade médical, Biocompatibility ISO 10993, USP Class VI approbation
Applications
Médical
Disponibilité régionale
Amérique du nord, Europe, Asia Pacific, South and Central America, Proche-Orient/Afrique
Conditions générales
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.