Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox. Information about Biopolymers, a project by FH Hannover and M-Base Engineering & Software GmbH sponsored by Fachagentur Nachwachsende Rohstoffe (FNR).

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Bio-Flex® FX 1821 - PLA... - FKuR Kunststoff GmbH

Material Data Center offers the following functions for Bio-Flex® FX 1821:
unit conversion, PDF datasheet print, comparison with other plastics

Check here, which other Bio-Flex datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Informations produit
Biodegradable and home compostable polymer compound. Certified as home compostable according to EN 13432 (at ambient temperature) with a maximum thickness of 32 μm. Suitable for blown film applications.
Caractéristiques des transformations/physiquesValeurUnitéNorme du test
ISO Data
Indice de fluidité à chaud en volume, MVR 3 cm³/10min ISO 1133
Température 190 °C -
Charge 2.16 kg -
Indice de fluidité, MFI 3.7 g/10min ISO 1133
Température 190 °C -
Charge 2.16 kg -
Propriétés thermiquesValeurUnitéNorme du test
ISO Data
Température de fusion, 10°C/min 155 °C ISO 11357-1/-3
Propriétés diversesValeurUnitéNorme du test
Masse volumique 1380 kg/m³ ISO 1183
Propriétés mécaniques (Grades film)ValeurUnitéNorme du test
ISO Data
Module en traction, parallèle 150 MPa ISO 527-3
Module en traction, perpend. 110 MPa ISO 527-3
Déformation au seuil, parallèle 500 % ISO 527-3
Déformation au seuil, perpend. 570 % ISO 527-3
Contrainte à la rupture, parallèle 23 MPa ISO 527-3
Contrainte à la rupture, perpend. 21 MPa ISO 527-3
Déformation maximale, parallèle 500 % ISO 527-3
Déformation maximale, perpend. 570 % ISO 527-3
Type d'extrusion soufflage - -
Epaisseur des eprouvettes 0.03 mm -
Recommandations pour la transformation ExtrusionValeurUnitéNorme du test
Type of extrusion blown - -
Pré-séchage - température 60 °C -
Pré-séchage - temps 2 - 4 h -
Température de la matière fondue 190 °C -
Température - Zone d'alimentation 60 °C -
Zone 1 160 °C -
Zone 2 165 °C -
Zone 3 170 °C -
Zone 4 175 °C -
Température de la buse 180 °C -
Caractéristiques
Transformation
Extrusion a film soufflé, Extrusion de films
Conditionnement
Granulés, Blanc
Propriétés spéciales
Opaque
Certifications
Contient des ressources renouvelables, Biodégradables, Contact alimentaire, Compostable ISO 13432 (producteur), Compostable ISO 13432 (certificat)
Applications
Emballage, Jouets
Disponibilité régionale
Amérique du nord, Europe, Asia Pacific, South and Central America, Proche-Orient/Afrique
Conditions générales
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.