Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of CELCON® M90 - POM - Celanese

Material Data Center offers the following functions for CELCON® M90:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, cooling time calculation, parameters for material models, CAE Interfaces

Check here, which other Celcon datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Caractéristiques des transformations/physiquesValeurUnitéNorme du test
ISO Data
Indice de fluidité à chaud en volume, MVR 8 cm³/10min ISO 1133
Température 190 °C -
Charge 2.16 kg -
Retrait au moulage, parallèle 2.0 % ISO 294-4, 2577
Retrait au moulage, perpendiculaire 1.9 % ISO 294-4, 2577
Densité du fondu 1200 kg/m³ -
Conductivité thermique du fondu 0.155 W/(m K) -
Chaleur spécifique du fondu 2210 J/(kg K) -
Diffusivité thermique 4.85E-8 m²/s -
Température d'éjection 140 °C -
Propriétés mécaniquesValeurUnitéNorme du test
ISO Data
Module en traction 2760 MPa ISO 527
Contrainte d'écoulement 65 MPa ISO 527
Déformation au seuil d'écoulement 10 % ISO 527
Résistance au choc Charpy, +23°C 188 kJ/m² ISO 179/1eU
Résistance au choc Charpy, -30°C 181 kJ/m² ISO 179/1eU
Résistance au choc Charpy (entaillé), +23°C 6 kJ/m² ISO 179/1eA
Résistance au choc Charpy (entaillé), -30°C 6 kJ/m² ISO 179/1eA
Propriétés thermiquesValeurUnitéNorme du test
ISO Data
Température de fusion, 10°C/min 166 °C ISO 11357-1/-3
Température de fléchissement s/chrg, 1.80 MPa 101 °C ISO 75-1/-2
Température de fléchissement s/chrg, 0.45 MPa 158 °C ISO 75-1/-2
Coeffic. de dilatation therm. linéique, parallèle 120 E-6/K ISO 11359-1/-2
Coeffic. de dilatation therm. linéique, perpend. 120 E-6/K ISO 11359-1/-2
Propriétés électriquesValeurUnitéNorme du test
ISO Data
Résistivité transversale 8E12 Ohm*m IEC 62631-3-1
Résistivité superficielle >1E15 Ohm IEC 62631-3-2
Propriétés diversesValeurUnitéNorme du test
Absorption d'eau 0.75 % Sim. to ISO 62
Absorption d'humidité 0.2 % Sim. to ISO 62
Masse volumique 1410 kg/m³ ISO 1183
Recommandations pour la transformation Moulage par injectionValeurUnitéNorme du test
Pré-séchage - température 80 °C -
Pré-séchage - temps 3 h -
L'humidité de traitement ≤0.35 % -
Température de la matière fondue 182 - 199 °C -
Température du moule 82 - 93 °C -
Fonctions
Contrainte / Déformation , CELCON® M90, POM, Celanese
Module sécant / Déformation , CELCON® M90, POM, Celanese
Contrainte / Déformation (isochrone) 23°C, CELCON® M90, POM, Celanese
Module de fluage / Temps 23°C, CELCON® M90, POM, Celanese
Courbe de fluage 23°C, CELCON® M90, POM, Celanese
Contrainte / Déformation (isochrone) 40°C, CELCON® M90, POM, Celanese
Module de fluage / Temps 40°C, CELCON® M90, POM, Celanese
Courbe de fluage 40°C, CELCON® M90, POM, Celanese
Caractéristiques
Transformation
Moulage par injection, Extrusion de films, Extrusion de profilés, Extrusion de plaques, Extrusion (autres), Soufflage, Calandrage
Conditionnement
Granulés
Caractéristiques
Copolymère
Disponibilité régionale
Amérique du nord, Europe, Asia Pacific, South and Central America, Proche-Orient/Afrique
Autres informations
Moulages par injection
Drying is generally not required because Celcon® and Hostaform® acetal copolymers are not hydroscopic nor are they degraded by moisture during processing. Excessive moisture can lead to splay (silver streaking) in molded parts. For better uniformity in molding especially when using regrind or material that has been stored in containers open to the atmosphere, recommended drying conditions are 80 C (180 F) for 3hours. Desiccant hopper dryers are not required. Maximum water content = 0.35%
Standard reciprocating screw injection molding machines with a high compression screw (minimum 3:1 and preferably 4:1) and low back pressure (0.35 Mpa/50 PSI) are favored. Using a low compression screw (I.E. general purpose 2:1 compression ratio) can result in unmelted particles and poor melt homogeneity. Using a high back pressure to make up for a low compression ratio may lead to excessive shear heating and deterioration of the material.

Melt Temperature: Preferred range 182-199 C (360-390 F). Melt temperature should never exceed 230 C (450 F).

Mold Surface Temperature: Preferred range 82-93 C (180-200 F) especially with wall thickness less than 1.5 mm (0.060 in.). May require mold temperature as high as 120 C (250 F) to reproduce mold surface or to assure minimal molded in stress. Wall thickness greater than 3mm (1/8 in.) may use a cooler (65 C/150 F) mold surface temperature and wall thickness over 6mm (1/4 in.) may use a cold mold surface down to 25 C (80 F). In general, mold surface temperatures lower than 82 C (180 F) may hinder weld line formation and produce a hazy surface or a surface with flow lines, pits and other included defects that can hinder part performance.
Postprocessing conditioning and moisturizing are not required. It may be necessary to fixture large or complicated parts with varying wall thickness to prevent warpage while cooling to ambient temperature.
Extrusion de films
Drying is generally not required because Celcon materials are not hydroscopic nor are they degraded by moisture during processing. Excessive moisture can cause surface defects on the extruded film. For better uniformity especially when using regrind or material that has been stored in containers open to the atmosphere, recommended drying conditions are 3 Hrs. at 80 C (180 F). Desiccant hopper dryers are not required. Max. moisture content = 0.35%.
Standard extruders with a length to diameter ratio of at least 20:1 are recommended. The screw should be a high compression ratio of at least 3:1 and preferably 4:1 to assure good melting and melt homogeneity. The design should be approximately 35% each for feed and metering sections with the remaining 30% as the transition zone.

Melt temperature: 160-220 C (320-430 F)
Postprocessing conditioning or moisturizing is not required.
Extrusion (autres)
Drying is generally not required because Celcon materials are not hydroscopic nor are they degraded by moisture during processing. Excessive moisture can cause surface defects. For better uniformity especially when using regrind or material that has been stored in containers open to the atmosphere, recommended drying is 3 hours at 80 C (180 F). Desiccant hopper dryers are not required. Max. moisture content = 0.35%
Standard extruders with a length to diameter ratio of at least 20:1 are recommended. The screw should be a high compression ratio of at least 3:1 and preferably 4:1 to assure good melting and uniform melt homogeneity. The design should be approximately 35% each for the feed and metering sections with the remaining 30% as transition zone.

Melt temperature 180-220 C (355-430F)
Postprocessing conditioning or moisturizing are not required. For thick walled sections (>3mm or 1/8 in.), annealing is recommended to reduce internal stresses.

Annealing temperature: 130-140 C (265-285 F)

Annealing time: 10 min/mm thickness
Extrusion de profilés
Drying is generally not required because Celcon materials are not hydroscopic nor are they degraded by moisture during processing. Excessive moisture can cause surface defects on the extrusion. For better uniformity especially when using regrind or material that has been stored in containers open to the atmosphere, recommended drying conditions are 3 Hrs. at 80 C (180 F). Desiccant hopper dryers are not required. Max. moisture content = 0.035%.
Standard extruders with a length to diameter ratio of at least 20:1 are recommended. The screw should be a high compression ratio of at least 3:1 and preferably 4:1 to assure good melting and melt homogeneity. The design should be approximately 35% each for feed and metering sections with the remaining 30% as the transition zone.

Melt temperature: 180-220 C (360-430 F).
Postprocessing or moisturizing is not required. For thick walled extrusions (>3 mm or 1/8 in.), annealing is recommended to reduce internal stresses.

Annealing temperature: 130-140 C (265-285 F)
Annealing time: 10 min/mm thickness
Extrusion de feuilles
Drying is generally not required because Celcon materials are not hydroscopic nor are they degraded by moisture during processing. Excessive moisture can lead to surface defects. For better uniformity in sheet extrusion especially when using regrind or material that has been stored in containers open to the atmosphere, recommended drying is 3 hours at 80 C (180 F). Desiccant hopper dryers are not required. Max. water content = 0.35%.
Standard extruders with a length to diameter ratio of at least 20:1 are recommended. The screw should be a high compression ratio (at least 3:1 and preferably 4:1) to assure good melting and uniform melt homogeneity. The screw design should be approximately 35% each for the feed and metering sections with the remaining 30% as the transition zone.

Melt temperature 180-190 C (355-375 F).
Postprocessing conditioning or moisturizing is not required. For thick walled sections (>3mm or 1/8 in.), annealing is recommended to reduce internal stresses.

Annealing temperature: 130-140 C (265-285 F)

Annealing time: 10 min/mm wall thickness
Soufflage
Consult product information services.
Consult product information services.
Consult product information services.
Calandrage
Consult product information services.
Consult product information services.
Consult product information services.
Conditions générales
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.