Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Makrolon® DQ5142 RE - PC - Covestro Deutschland AG

Material Data Center offers the following functions for Makrolon® DQ5142 RE:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Makrolon datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Caractéristiques des transformations/physiquesValeurUnitéNorme du test
ISO Data
Indice de fluidité à chaud en volume, MVR 34 cm³/10min ISO 1133
Température 300 °C -
Charge 1.2 kg -
Retrait au moulage, parallèle 0.7 % ISO 294-4, 2577
Retrait au moulage, perpendiculaire 0.7 % ISO 294-4, 2577
Propriétés mécaniquesValeurUnitéNorme du test
ISO Data
Module en traction 2300 MPa ISO 527
Contrainte d'écoulement 65 MPa ISO 527
Déformation au seuil d'écoulement 6 % ISO 527
Déformation nominale à la rupture >50 % ISO 527
Contrainte à la rupture 60 MPa ISO 527
Déformation à la rupture 110 % ISO 527
Résistance au choc Charpy, +23°C N kJ/m² ISO 179/1eU
Résistance au choc Charpy, -30°C N kJ/m² ISO 179/1eU
Résistance au choc Charpy (entaillé), +23°C, 3mm 12 kJ/m² ISO 179/1eA
Type de défaillance C - -
Résistance au choc Charpy (entaillé), -30°C, 3mm 12 kJ/m² ISO 179/1eA
Type de défaillance C - -
Perforation - force maximum, +23°C 4900 N ISO 6603-2
Perforation - force maximum, -30°C 5900 N ISO 6603-2
Perforation - Energie, +23°C 44 J ISO 6603-2
Perforation - Energie, -30°C 50 J ISO 6603-2
Ball indentation hardness 120 MPa ISO 2039-1
Propriétés thermiquesValeurUnitéNorme du test
ISO Data
Température de fléchissement s/chrg, 1.80 MPa 120 °C ISO 75-1/-2
Température de fléchissement s/chrg, 0.45 MPa 134 °C ISO 75-1/-2
Température de ramolliss. Vicat, B 140 °C ISO 306
Inflammabilité pr. épaisseur h V-2 class IEC 60695-11-10
Epaisseur de l'éprouvette 0.8 mm -
Yellow Card disponible oui - -
Glow Wire Flammability Index (GWFI) 850 °C IEC 60695-2-12
GWFI - thickness tested (1) 0.75 mm -
Glow Wire Flammability Index (GWFI) 850 °C IEC 60695-2-12
GWFI - thickness tested (2) 1.5 mm -
Glow Wire Flammability Index (GWFI) 930 °C IEC 60695-2-12
GWFI - thickness tested (3) 3 mm -
Glow Wire Ignition Temperature (GWIT) 850 °C IEC 60695-2-13
GWIT - thickness tested (1) 0.75 mm -
Glow Wire Ignition Temperature (GWIT) 850 °C IEC 60695-2-13
GWIT - thickness tested (2) 1.5 mm -
Glow Wire Ignition Temperature (GWIT) 850 °C IEC 60695-2-13
GWIT - thickness tested (3) 3 mm -
Propriétés optiquesValeurUnitéNorme du test
ISO Data
Haze 100[1] - ISO 14782
Transmittance 80[1] % ISO 13468-1, -2
1: 1 mm
Propriétés diversesValeurUnitéNorme du test
Absorption d'eau 0.3 % Sim. to ISO 62
Absorption d'humidité 0.12 % Sim. to ISO 62
Masse volumique 1200 kg/m³ ISO 1183
Préparation et conditionnement des éprouvettesValeurUnitéNorme du test
ISO Data
Injection, température de la matière fondue 280 °C ISO 294
Injection, température du moule 80 °C ISO 294
injection, vitesse d'injection 200 mm/s ISO 294
Recommandations pour la transformation Moulage par injectionValeurUnitéNorme du test
Pré-séchage - température 120 °C -
Pré-séchage - temps 2 - 3 h -
L'humidité de traitement ≤0.02 % -
Température de la matière fondue 250 - 300 °C -
Température du moule 80 - 120 °C -
Zone 1 230 - 240 °C -
Zone 2 250 - 260 °C -
Zone 3 260 - 270 °C -
Température de la buse 260 - 270 °C -
Contre-pression 5 - 15 MPa -
Caractéristiques
Transformation
Moulage par injection
Additifs
Agent de démoulage
Propriétés spéciales
Stabilisé aux intempéries, Translucent
Caractéristiques
Light Diffusing
Certifications
Contient des ressources renouvelables, ISCC Plus
Disponibilité régionale
Amérique du nord, Europe, Asia Pacific, South and Central America, Proche-Orient/Afrique
Conditions générales
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.