Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultrafuse PAHT CF15 - PA*-CF15 - BASF

Material Data Center offers the following functions for Ultrafuse PAHT CF15:
unit conversion, PDF datasheet print, comparison with other plastics

Check here, which other Ultrafuse datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Caractéristiques des transformations/physiquessec / condUnitéNorme du test
ISO Data
Indice de fluidité à chaud en volume, MVR 42.2 / * cm³/10min ISO 1133
Température 275 / * °C -
Charge 5 / * kg -
Propriétés thermiquessec / condUnitéNorme du test
ISO Data
Température de fusion, 10°C/min 234 / * °C ISO 11357-1/-3
Température de transition vitreuse, 10°C/min 70 / * °C ISO 11357-1/-2
Température de fléchissement s/chrg, 1.80 MPa 92 / * °C ISO 75-1/-2
Température de fléchissement s/chrg, 0.45 MPa 145 / * °C ISO 75-1/-2
Propriétés diversessec / condUnitéNorme du test
Masse volumique 1230 / 1230 kg/m³ ISO 1183
3D Datasec / condUnitéNorme du test
Other Standards[S]
Module en traction, flat 8390 / 5050 MPa ISO 527
Module en traction, upright 3530 / 2460 MPa ISO 527
Résistance à la traction, flat 103 / 62.9 MPa ISO 527
Résistance à la traction, upright 18.2 / 19.1 MPa ISO 527
Déformation à la rupture, flat 1.8 / 2.9 % ISO 527
Déformation à la rupture, upright 0.5 / 0.8 % ISO 527
Module de flexion, flat 8260 / 6060 MPa ISO 178
Module de flexion, on-edge 7670 / 6260 MPa ISO 178
Module de flexion, upright 2710 / 2190 MPa ISO 178
Résistance à la flexion, flat 161 / 125 MPa ISO 178
Résistance à la flexion, on-edge 172 / 122 MPa ISO 178
Résistance à la flexion, upright 50.8 / 56 MPa ISO 178
Résistance au choc Charpy, +23°C, flat 20.6 / 21.9 kJ/m² ISO 179/1eU
Résistance au choc Charpy, +23°C, on-edge 19.3 / 20.4 kJ/m² ISO 179/1eU
Résistance au choc Charpy, +23°C, upright 2.9 / 2.8 kJ/m² ISO 179/1eU
Résistance au choc Charpy (entaillé), +23°C, flat 4.8 / 5.1 kJ/m² ISO 179/1eA
Résistance au choc Charpy (entaillé), +23°C, on-edge 3.9 / 5.3 kJ/m² ISO 179/1eA
Résistance au choc Charpy (entaillé), +23°C, upright 1.3 / 1.6 kJ/m² ISO 179/1eA
Résistance au choc Izod, +23°C, flat 16.4 / 16.3 kJ/m² ISO 180/1U
Résistance au choc Izod, +23°C, on-edge 18.1 / 15.1 kJ/m² ISO 180/1U
Résistance au choc Izod, +23°C, upright 2.9 / 4.1 kJ/m² ISO 180/1U
Résistance au choc Izod avec entaille, +23°C, flat 4.9 / 6.5 kJ/m² ISO 180/1A
Résistance au choc Izod avec entaille, +23°C, on-edge 5.1 / 5.8 kJ/m² ISO 180/1A
S: These properties are reported by the producer according standards that are different to our defaults.
Caractéristiques
Transformation
Additive Manufacturing
Conditionnement
Monofilament
Propriétés spéciales
Stabilisé à la chaleur
Résistance Chimique
Résistance chimique générale
Disponibilité régionale
Amérique du nord, Europe, South and Central America
Conditions générales
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.