Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultraform® H2320 008 AT - POM - BASF

Material Data Center offers the following functions for Ultraform® H2320 008 AT:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultraform datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Testo del prodotto
High-molecular-weight grade with somewhat increased flowability for injection molding of relatively thick-walled moldings.

Abbreviated designation according to ISO 1043-1: POM
Designation according to ISO 29988-POM-K,,M-GNR,1-2
Caratteristiche FisicheValoreUnitáNorma del test
ISO Data
Indice di fusione di volume, MVR 2.9 cm³/10min ISO 1133
Temperatura 190 °C -
Carico 2.16 kg -
Ritiro di stampaggio, parallelo 2.1 % ISO 294-4, 2577
Ritiro di stampaggio, perpendicolare 2.1 % ISO 294-4, 2577
Conduttività termica del fuso 0.14 W/(m K) -
Capacità termica specifica del fuso 2800 J/(kg K) -
Temperatura di estrazione 110 °C -
Proprietà MeccanicheValoreUnitáNorma del test
ISO Data
Modulo a trazione 2600 MPa ISO 527
Carico unitario a trazione 62 MPa ISO 527
Deformazione a snervamento 11 % ISO 527
Deformazione nominale a rottura 30 % ISO 527
Modulo di scorrimento a trazione, 1h 1800 MPa ISO 899-1
Modulo di scorrimento a trazione, 1000h 1300 MPa ISO 899-1
Resistenza all'urto Charpy, +23°C 270 kJ/m² ISO 179/1eU
Resistenza all'urto Charpy, -30°C 260 kJ/m² ISO 179/1eU
Resistenzia all'urto Charpy con intaglio, +23°C 6.5 kJ/m² ISO 179/1eA
Resistenzia all'urto Charpy con intaglio, -30°C 5.5 kJ/m² ISO 179/1eA
Proprietà TermicheValoreUnitáNorma del test
ISO Data
Temperatura di fusione, 10°C/min 165 °C ISO 11357-1/-3
Temp.di inflessione sotto carico, 1.80 MPa 95 °C ISO 75-1/-2
Temp.di inflessione sotto carico, 0.45 MPa 156 °C ISO 75-1/-2
Temp.di rammollimento Vicat, B 150 °C ISO 306
Coeff.di dilatazione termica lin., parallelo 120 E-6/K ISO 11359-1/-2
Reaz. al fuoco spess.nom. 1.5mm HB class IEC 60695-11-10
Spessore provato 1.6 mm -
Yellow Card disponibile - -
Reazione al fuoco a spessore h HB class IEC 60695-11-10
Spessore provato 0.8 mm -
Yellow Card disponibile - -
Indice di ossigeno 15 % ISO 4589-1/-2
Proprietà ElettricheValoreUnitáNorma del test
ISO Data
Costante dielettrica relativa, 100Hz 3.8 - IEC 62631-2-1
Costante dielettrica relativa, 1MHz 3.8 - IEC 62631-2-1
Fattore di dissipazione, 100Hz 10 E-4 IEC 62631-2-1
Fattore di dissipazione, 1MHz 50 E-4 IEC 62631-2-1
Resistività volumica 1E11 Ohm*m IEC 62631-3-1
Resistività superficiale 1E13 Ohm IEC 62631-3-2
Rigidità dielettrica 40 kV/mm IEC 60243-1
Res. Alle correnti striscianti superficiali 600 - IEC 60112
Altre ProprietàValoreUnitáNorma del test
Assorbimento d'acqua 0.95 % Sim. alla ISO 62
Assorbimento d'umidità 0.25 % Sim. alla ISO 62
Massa volumica 1410 kg/m³ ISO 1183
Preparazione ProvetteValoreUnitáNorma del test
ISO Data
Stamp. ad Iniezione, temp. di fusione 200 °C ISO 294
Stamp. ad Iniezione, temperatura dello stampo 90 °C ISO 294
Stamp. ad Iniezione, velocità media d'iniezione 200 mm/s ISO 294
Raccomandazione de Processabilità Stampaggio ad IniezioneValoreUnitáNorma del test
Pre-essiccamento - Temperatura 100 °C -
Pre-essiccamento - Tempo 3 h -
Umidità del Processo ≤0.2 % -
Temperatura di fusione 190 - 230 °C -
Temperatura dello stampo 60 - 120 °C -
Funzioni
Volume specifico-temperatura (pvT) , Ultraform® H2320 008 AT, POM, BASF
Caratteristiche
Processabilità e Forma di Forni
Stampaggio ad Iniezione, Estrusione Film, Estrusione Profilati, Estrusione di Lastre/Fogli, Altre Estrusioni
Forma fisica disponibile
Pellet
Additivi
Agente di distacco
Caratteristiche
Copolimero
Disponibilità geografica
Altre informazioni
Stampaggio ad Iniezione
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
injection molding, Melt temperature, range: 190 - 230 °C
injection molding, Melt temperature, recommended: 200 °C
injection molding, Mold temperature, range: 60 - 120 °C
injection molding, Mold temperature, recommended: 90 °C
injection molding, Dwell time, thermoplastics: 10 min
Estrusione Film
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
Extrusion, Blown film, Melt temperature: 175 - 180 °C
Extrusion, Flat film, Melt temperature: 175 - 180 °C

Processing

Ultraform can be processed to particular advantage using three-section screws having a total length L of 20 - 25 D and a constant pitch of about 1 D. However short-compression zone screws may also be used.

Pretreatment

Granules or pellets in original packaging can be processed without any special pretreatment. Granules or pellets which have become moist due to prolonged or incorrect storage (e.g. by formation of condensed water) must be dried in dehumidifying or recirculating air dryers for approx. 3 hours at about 100 - 110 °C. The moisture content should not exceed 0.2 %.

Postprocessing

Due to the different solidification and cooling of the melt which varies according to time and place stresses may arise, especially in the case of large wall thicknesses. These stresses can be removed by subsequent heat treatment. Tempering is essential when high demands are placed on dimensional stability. It can be carried out in air, liquid wax or oil at temperatures of 130 - 150, usually 140 - 145 °C. Lower temperatures are not effective. Duration: 10 minutes per 1 mm wall thickness.
Altre Estrusioni
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
Extrusion, Prepreg, Melt temperature: 175 - 180 °C
Extrusion, Pipes, Melt temperature: 175 - 180 °C
Extrusion, cable sheathing, Melt temperature: 175 - 180 °C

Processing

Ultraform can be processed to particular advantage using three-section screws having a total length L of 20 - 25 D and a constant pitch of about 1 D. However short-compression zone screws may also be used.

Pretreatment

Granules or pellets in original packaging can be processed without any special pretreatment. Granules or pellets which have become moist due to prolonged or incorrect storage (e.g. by formation of condensed water) must be dried in dehumidifying or recirculating air dryers for approx. 3 hours at about 100 - 110 °C. The moisture content should not exceed 0.2 %.

Postprocessing

Due to the different solidification and cooling of the melt which varies according to time and place stresses may arise, especially in the case of large wall thicknesses. These stresses can be removed by subsequent heat treatment. Tempering is essential when high demands are placed on dimensional stability. It can be carried out in air, liquid wax or oil at temperatures of 130 - 150, usually 140 - 145 °C. Lower temperatures are not effective. Duration: 10 minutes per 1 mm wall thickness.
Estrusione di Profilati
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
Extrusion, Profiles, Melt temperature: 175 - 180 °C

Processing

Ultraform can be processed to particular advantage using three-section screws having a total length L of 20 - 25 D and a constant pitch of about 1 D. However short-compression zone screws may also be used.

Pretreatment

Granules or pellets in original packaging can be processed without any special pretreatment. Granules or pellets which have become moist due to prolonged or incorrect storage (e.g. by formation of condensed water) must be dried in dehumidifying or recirculating air dryers for approx. 3 hours at about 100 - 110 °C. The moisture content should not exceed 0.2 %.

Postprocessing

Due to the different solidification and cooling of the melt which varies according to time and place stresses may arise, especially in the case of large wall thicknesses. These stresses can be removed by subsequent heat treatment. Tempering is essential when high demands are placed on dimensional stability. It can be carried out in air, liquid wax or oil at temperatures of 130 - 150, usually 140 - 145 °C. Lower temperatures are not effective. Duration: 10 minutes per 1 mm wall thickness.
Estrusione Lastre/Fogli
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
Extrusion, Plates, Melt temperature: 175 - 180 °C

Processing

Ultraform can be processed to particular advantage using three-section screws having a total length L of 20 - 25 D and a constant pitch of about 1 D. However short-compression zone screws may also be used.

Pretreatment

Granules or pellets in original packaging can be processed without any special pretreatment. Granules or pellets which have become moist due to prolonged or incorrect storage (e.g. by formation of condensed water) must be dried in dehumidifying or recirculating air dryers for approx. 3 hours at about 100 - 110 °C. The moisture content should not exceed 0.2 %.

Postprocessing

Due to the different solidification and cooling of the melt which varies according to time and place stresses may arise, especially in the case of large wall thicknesses. These stresses can be removed by subsequent heat treatment. Tempering is essential when high demands are placed on dimensional stability. It can be carried out in air, liquid wax or oil at temperatures of 130 - 150, usually 140 - 145 °C. Lower temperatures are not effective. Duration: 10 minutes per 1 mm wall thickness.
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.