Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultraform® W2320 003 TR AT - POM - BASF

Material Data Center offers the following functions for Ultraform® W2320 003 TR AT:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultraform datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Testo del prodotto
Very free-flowing grade for injection molding with special lubricant to minimize friction,wear, stick-slip and squeaking.

Abbreviated designation according to ISO 1043-1: POM
Designation according to ISO 29988-POM-K,,M-GNRS2,5-2
Caratteristiche FisicheValoreUnitáNorma del test
ISO Data
Indice di fusione di volume, MVR 25 cm³/10min ISO 1133
Temperatura 190 °C -
Carico 2.16 kg -
Ritiro di stampaggio, parallelo 2.0 % ISO 294-4, 2577
Ritiro di stampaggio, perpendicolare 1.9 % ISO 294-4, 2577
Proprietà MeccanicheValoreUnitáNorma del test
ISO Data
Modulo a trazione 2500 MPa ISO 527
Carico unitario a trazione 50 MPa ISO 527
Deformazione a snervamento 5.5 % ISO 527
Deformazione nominale a rottura 37 % ISO 527
Resistenza all'urto Charpy, +23°C 110 kJ/m² ISO 179/1eU
Resistenza all'urto Charpy, -30°C 95 kJ/m² ISO 179/1eU
Resistenzia all'urto Charpy con intaglio, +23°C 5 kJ/m² ISO 179/1eA
Resistenzia all'urto Charpy con intaglio, -30°C 4.4 kJ/m² ISO 179/1eA
Proprietà TermicheValoreUnitáNorma del test
ISO Data
Temperatura di fusione, 10°C/min 167 °C ISO 11357-1/-3
Temp.di inflessione sotto carico, 1.80 MPa 92 °C ISO 75-1/-2
Coeff.di dilatazione termica lin., parallelo 125 E-6/K ISO 11359-1/-2
Proprietà ElettricheValoreUnitáNorma del test
ISO Data
Costante dielettrica relativa, 100Hz 3.5 - IEC 62631-2-1
Costante dielettrica relativa, 1MHz 3.5 - IEC 62631-2-1
Fattore di dissipazione, 100Hz 9 E-4 IEC 62631-2-1
Fattore di dissipazione, 1MHz 55 E-4 IEC 62631-2-1
Resistività volumica 1E11 Ohm*m IEC 62631-3-1
Resistività superficiale 1E14 Ohm IEC 62631-3-2
Res. Alle correnti striscianti superficiali 600 - IEC 60112
Altre ProprietàValoreUnitáNorma del test
Assorbimento d'acqua 0.8 % Sim. alla ISO 62
Assorbimento d'umidità 0.2 % Sim. alla ISO 62
Massa volumica 1380 kg/m³ ISO 1183
Raccomandazione de Processabilità Stampaggio ad IniezioneValoreUnitáNorma del test
Pre-essiccamento - Temperatura 100 °C -
Pre-essiccamento - Tempo 3 h -
Umidità del Processo ≤0.2 % -
Temperatura di fusione 190 - 230 °C -
Temperatura dello stampo 60 - 120 °C -
Funzioni
Viscosità-Velocità di taglio , Ultraform® W2320 003 TR AT, POM, BASF
Sforzo di taglio-Velocità di taglio , Ultraform® W2320 003 TR AT, POM, BASF
Modulo dinamico a taglio-temperatura , Ultraform® W2320 003 TR AT, POM, BASF
Sforzi-deformazione , Ultraform® W2320 003 TR AT, POM, BASF
Modulo secante-deformazione , Ultraform® W2320 003 TR AT, POM, BASF
Sforzi-deformazioni (isocrona) 23°C, Ultraform® W2320 003 TR AT, POM, BASF
Modulo di scorrimento-tempo 23°C, Ultraform® W2320 003 TR AT, POM, BASF
Curva di scorrimento 23°C, Ultraform® W2320 003 TR AT, POM, BASF
Sforzi-deformazioni (isocrona) 40°C, Ultraform® W2320 003 TR AT, POM, BASF
Modulo di scorrimento-tempo 40°C, Ultraform® W2320 003 TR AT, POM, BASF
Curva di scorrimento 40°C, Ultraform® W2320 003 TR AT, POM, BASF
Sforzi-deformazioni (isocrona) 60°C, Ultraform® W2320 003 TR AT, POM, BASF
Modulo di scorrimento-tempo 60°C, Ultraform® W2320 003 TR AT, POM, BASF
Curva di scorrimento 60°C, Ultraform® W2320 003 TR AT, POM, BASF
Sforzi-deformazioni (isocrona) 80°C, Ultraform® W2320 003 TR AT, POM, BASF
Modulo di scorrimento-tempo 80°C, Ultraform® W2320 003 TR AT, POM, BASF
Curva di scorrimento 80°C, Ultraform® W2320 003 TR AT, POM, BASF
Sforzi-deformazioni (isocrona) 100°C, Ultraform® W2320 003 TR AT, POM, BASF
Modulo di scorrimento-tempo 100°C, Ultraform® W2320 003 TR AT, POM, BASF
Curva di scorrimento 100°C, Ultraform® W2320 003 TR AT, POM, BASF
Sforzi-deformazioni (isocrona) 120°C, Ultraform® W2320 003 TR AT, POM, BASF
Modulo di scorrimento-tempo 120°C, Ultraform® W2320 003 TR AT, POM, BASF
Curva di scorrimento 120°C, Ultraform® W2320 003 TR AT, POM, BASF
Volume specifico-temperatura (pvT) , Ultraform® W2320 003 TR AT, POM, BASF
Modulo a taglio-temperatura , Ultraform® W2320 003 TR AT, POM, BASF
Caratteristiche
Processabilità e Forma di Forni
Stampaggio ad Iniezione
Forma fisica disponibile
Pellet
Additivi
Lubrificanti, Agente di distacco
Caratteristiche
Grado tribologico
Disponibilità geografica
Altre informazioni
Stampaggio ad Iniezione
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
injection molding, Melt temperature, range: 190 - 230 °C
injection molding, Melt temperature, recommended: 210 °C
injection molding, Mold temperature, range: 60 - 120 °C
injection molding, Mold temperature, recommended: 90 °C
injection molding, Dwell time, thermoplastics: 10 min

Processing

Usual single-flighted three-section screws with an effective screw length of at least 15 D, better 20 - 23 D are suitable for the injection molding of Ultraform.

Pretreatment

Granules or pellets in original packaging can be processed without any special pretreatment. Granules or pellets which have become moist due to prolonged or incorrect storage (e.g. by formation of condensed water) must be dried in dehumidifying or recirculating air dryers for approx. 3 hours at about 100 - 110 °C. The moisture content should not exceed 0.2 %.


Postprocessing

If parts were produced at a comparatively low mold temperature (e.g. in order to obtain short cycle times) and must not change their geometry in use thermal postprocessing inducing dimensional changes by postcrystallization may be necessary. In such cases parts should be stored in an oven with recirculated air at temperatures of 100 - 130 °C until dimensions don't change significantly any further. The time needed for this has to be determined experimentally.
Resistenza chimica
Acidi
Acido acetico (5% da massa) (23°C)
Acido lattico (10% da massa) (23°C)
Acido cloridrico (36% da massa) (23°C)
Acido nitrico (40% da massa) (23°C)
Acido solforico (38% da massa) (23°C)
Acido solforico (5% da massa) (23°C)
Soluzione acida cromica (40% da massa) (23°C)
Basi
Soluzione dell' idrossido del sodio (35% da massa) (23°C)
Soluzione dell' idrossido del sodio (1% da massa) (23°C)
Soluzione dell' idrossido di ammonio (10% da massa) (23°C)
Alcool
Alcool di isopropile (23°C)
Metanolo (23°C)
Etanolo (23°C)
Idrocarburi
n-Hexane (23°C)
Toluene (23°C)
isoottano (23°C)
Chetoni
Acetone (23°C)
Eteri
Etere Etilico (23°C)
Oli minerali
Olio multigrade del motore di SAE 10W40 (130°C)
Olio dell' ipoide-ingranaggio di SAE 80/90 (130°C)
Combustibili Standard
Liquido 1 di ISO 1817 (60°C)
Liquido 2 di ISO 1817 (60°C)
Liquido 3 di ISO 1817 (60°C)
Liquido 4 di ISO 1817 (60°C)
Combust. stand. senza alcool (pref. ISO 1817 liquido C) (23°C)
Combust. stand. con alcool (pref. ISO 1817 liquido 4) (23°C)
Combustibile diesel (pref. ISO 1817 liquido F) (23°C)
Combustibile diesel (pref. ISO 1817 liquido F) (>90°C)
Soluzioni saline
Soluzione del cloruro di sodio (10% da massa) (23°C)
Soluzione dell' ipoclorito del sodio (10% da massa) (23°C)
Soluzione del carbonato di sodio (20% da massa) (23°C)
Soluzione del carbonato di sodio (2% da massa) (23°C)
Altri
Acetato etilico (23°C)
Perossido di idrogeno (23°C)
Liquido di freno del DOT N° 4 (130°C)
Glicol etilenico (50% da massa) in acqua (108°C)
acido oleico 50% + olio di oliva 50% (23°C)
Acqua (23°C)
Acqua deionizzata (90°C)
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.