Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAMID® Care ME71 - TPA - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAMID® Care ME71:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vestamid datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Testo del prodotto
Polyamide 12 elastomer molding compounds

VESTAMID® Care ME71 is free of plasticizers and heat and light stabilized. VESTAMID® Care ME71 is resistant to body fluids and toxicologically safe.

VESTAMID® Care ME grades are flexible polyether block amides (PEBA) resins.

The advantages at a glance:
  • High flexibility & elasticity
  • Good rebound properties
  • High impact resistance
  • Excellent dimensional stability
  • High chemical resistance
  • Easy processability & colorability
  • Plasticizer-free
  • Gamma and EtO sterilization resistant
  • Tough and resilient

Biocompatibility of VESTAMID® Care ME

Biocompatiblity was tested following ISO10993-1 recommendations for a surface medical device with up to 30 days body contact.
 
The material fulfills the requirements of USP<88> class VI.
 
Tests were performed by independent, certified laboratories.

Biocompatibility tests for VESTAMID® Care:
Standard Description
ASTM F756-08 Hemocompatibility
ISO 10993-5 Cytotoxicity
ISO 10993-10 Sensitization: Maximization test according to Magnusson and Kligman
ISO 10993-10 Irritation: Intracutaneous Reactivity
ISO 10993-11 Acute Systemic Toxicity
USP Class VI Acute Systemic Toxicity Intracutaneous Reactivity Muscle Implantation


Processing of VESTAMID® Care
For information about processing of VESTAMID®, please follow the general commendations about “Processing of VESTAMID® compounds”. 

The values presented are typical or average values, they do not constitute a specification. 

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM
OR VISIT OUR PRODUCT AT  WWW.EVONIK.COM/MEDICAL-TECHNOLOGY
Caratteristiche Fisichesecco/condUnitáNorma del test
ISO Data
Indice di fusione di volume, MVR 75 / * cm³/10min ISO 1133
Temperatura 240 / * °C -
Carico 2.16 / * kg -
Ritiro di stampaggio, parallelo 1.2 / * % ISO 294-4, 2577
Ritiro di stampaggio, perpendicolare 1.3 / * % ISO 294-4, 2577
Proprietà Meccanichesecco/condUnitáNorma del test
ISO Data
Modulo a trazione 1090 / 760 MPa ISO 527
Carico unitario a trazione 39 / 34 MPa ISO 527
Deformazione a snervamento 13 / 16 % ISO 527
Deformazione nominale a rottura >50 / >50 % ISO 527
Resistenza all'urto Charpy, +23°C N / N kJ/m² ISO 179/1eU
Resistenza all'urto Charpy, -30°C N / N kJ/m² ISO 179/1eU
Resistenzia all'urto Charpy con intaglio, +23°C 5 / 7 kJ/m² ISO 179/1eA
Type of failure C / C - -
Resistenzia all'urto Charpy con intaglio, -30°C 6 / 4 kJ/m² ISO 179/1eA
Type of failure C / C - -
Durezza Shore D 71 / * - ISO 7619-1
Proprietà Termichesecco/condUnitáNorma del test
ISO Data
Temperatura di fusione, 10°C/min 177 / * °C ISO 11357-1/-3
Temp.di inflessione sotto carico, 1.80 MPa 54 / * °C ISO 75-1/-2
Temp.di inflessione sotto carico, 0.45 MPa 111 / * °C ISO 75-1/-2
Temp.di rammollimento Vicat, B 137 / * °C ISO 306
Coeff.di dilatazione termica lin., parallelo 150 / * E-6/K ISO 11359-1/-2
Coeff.di dilatazione termica lin., perpend. 155 / * E-6/K ISO 11359-1/-2
Reaz. al fuoco spess.nom. 1.5mm HB / * class IEC 60695-11-10
Spessore provato 1.6 / * mm -
Proprietà Elettrichesecco/condUnitáNorma del test
ISO Data
Costante dielettrica relativa, 100Hz 4.5 / - - IEC 62631-2-1
Costante dielettrica relativa, 1MHz 3.2 / - - IEC 62631-2-1
Fattore di dissipazione, 100Hz 760 / - E-4 IEC 62631-2-1
Fattore di dissipazione, 1MHz 334 / - E-4 IEC 62631-2-1
Resistività volumica 4E12 / 2.9E11 Ohm*m IEC 62631-3-1
Altre Proprietàsecco/condUnitáNorma del test
Assorbimento d'acqua 1.5 / * % Sim. alla ISO 62
Assorbimento d'umidità 0.7 / * % Sim. alla ISO 62
Massa volumica 1010 / - kg/m³ ISO 1183
Preparazione ProvetteValoreUnitáNorma del test
ISO Data
Stamp. ad Iniezione, temp. di fusione 220 °C ISO 294
Stamp. ad Iniezione, temperatura dello stampo 35 °C ISO 294
Stamp. ad Iniezione, velocità media d'iniezione 200 mm/s ISO 294
Caratteristiche
Processabilità e Forma di Forni
Stampaggio ad Iniezione
Forma fisica disponibile
Pellet
Caratteristiche speciali
Alto urto o modificato all'urto, Stabilizzato o stabile alla luce, Stabilizzato o stabile al calore, Sterilizzabile, Sterilizzazione ad ossido di etilene (EtO), Gamma irradiation sterilization
Resistenza Chimica
Resistenza chimica generale
Certifications
Grado medico, Biocompatibility ISO 10993, Approvazione della USP class VI
Applicazioni
Medicale
Disponibilità geografica
Nord America, Europa, Asia Oceano Pacifico, South and Central America, Near East/Africa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.