Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAMID® DX9325 BK E70352 - PA612-GF40 - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAMID® DX9325 BK E70352:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vestamid datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Testo del prodotto
Heat-stabilized, glass fiber-reinforced, PA 612 compound for plastic-EPDM-rubber bonds

VESTAMID® DX9325 BK E70352 is a glass fiber-reinforced, PA 612 molding compound. The material contains about 40% glass fiber, an ageing protective agent and processing aid for a fast and even form filling. VESTAMID® DX9325 BK E70352 is especially suitable for the production of plastic and rubber composites. 

Parts of VESTAMID® DX9325 BK E70352 can be co-vulcanized with EPDM-rubbers without using any adhesives or adhesion promoters ("direct-bonding to rubber"). Because of its semi-crystalline morphology VESTAMID® DX9325 BK E70352 provides an excellent chemical resistance, e. g., against greases, oils, fuels and hydraulic fluids.

VESTAMID® DX9325 BK E70352 is supplied as cylindrical pellets ready for processing in moisture-proof bags.

Very important are predrying conditions. The material has to be handle as plasticized PA 612. The drying temperature should be not more than 80°C and the drying time at this temperature not more than 4h.
 
Pigmentation may affect values.

Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at temperatures not exceeding 30°C.

For information about processing of VESTAMID®, please follow the general commendations about “Processing of VESTAMID® compounds”. 

The values presented are typical or average values, they do not constitute a specification.

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM
OR VISIT OUR PRODUCT AT  WWW.VESTAMID.COM
Caratteristiche Fisichesecco/condUnitáNorma del test
ISO Data
Ritiro di stampaggio, parallelo 0.2 / * % ISO 294-4, 2577
Ritiro di stampaggio, perpendicolare 0.7 / * % ISO 294-4, 2577
Proprietà Meccanichesecco/condUnitáNorma del test
ISO Data
Modulo a trazione 10300 / - MPa ISO 527
Carico unitario a rottura 160 / - MPa ISO 527
Deformazione a rottura 4.4 / - % ISO 527
Resistenza all'urto Charpy, +23°C 100 / - kJ/m² ISO 179/1eU
Type of failure C / - - -
Resistenza all'urto Charpy, -30°C 104 / - kJ/m² ISO 179/1eU
Type of failure C / - - -
Resistenzia all'urto Charpy con intaglio, +23°C 18 / - kJ/m² ISO 179/1eA
Type of failure C / - - -
Resistenzia all'urto Charpy con intaglio, -30°C 16 / - kJ/m² ISO 179/1eA
Type of failure C / - - -
Proprietà Termichesecco/condUnitáNorma del test
ISO Data
Temp.di inflessione sotto carico, 1.80 MPa 200 / * °C ISO 75-1/-2
Temp.di inflessione sotto carico, 0.45 MPa 215 / * °C ISO 75-1/-2
Altre Proprietàsecco/condUnitáNorma del test
Massa volumica 1410 / - kg/m³ ISO 1183
Preparazione ProvetteValoreUnitáNorma del test
ISO Data
Stamp. ad Iniezione, temp. di fusione 260 °C ISO 294
Stamp. ad Iniezione, temperatura dello stampo 80 °C ISO 294
Stamp. ad Iniezione, velocità media d'iniezione 200 mm/s ISO 294
Caratteristiche
Processabilità e Forma di Forni
Stampaggio ad Iniezione
Forma fisica disponibile
Pellet, Nero
Additivi
Agente di distacco
Caratteristiche speciali
Stabilizzato o stabile alla luce, Stabilizzato o stabile al calore
Caratteristiche
Buona adesione
Resistenza Chimica
Resistenza chimica generale, Resistenza al grasso, Resistenza all’olio
Disponibilità geografica
Nord America, Europa, Asia Oceano Pacifico, South and Central America, Near East/Africa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.