Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAMID® L-GF15 - PA12-GF15 - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAMID® L-GF15:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Vestamid datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Testo del prodotto

Glass fibre reinforced (15%) PA12 resin for the injection moulding of rigid and tough parts


VESTAMID® L-GF15 NC is a glass fiber –reinforced heat stabilized Polyamide 12 for injection molding. The material contains about 15% glass fibers, an ageing protective agent and a processing aid for a fast and even form filling. Due to the reinforcement moldings from this compound exhibit a higher strength and good heat resistance, excellent for gear housings for electric window openers in cars.


Further advantages of VESTAMID® L-GF15 NC are the characterizing properties of PA12, e.g., low water absorption, good dimensional stability and nearly constant mechanical properties at changing ambient humidity.

  
VESTAMID® L-GF15 NC is supplied as cylindrical granules, ready for processing, in moisture-proof bags.

 
The use of colorants may change property values.


Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at temperatures not exceeding 30°C.


For information about processing of VESTAMID®, please follow the general commendations about “Processing of VESTAMID® compounds”. 
 

The values presented are typical or average values, they do not constitute a specification.

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM

OR VISIT OUR PRODUCT AT  WWW.VESTAMID.COM
Caratteristiche Fisichesecco/condUnitáNorma del test
ISO Data
Indice di fusione di volume, MVR 55 / * cm³/10min ISO 1133
Temperatura 275 / * °C -
Carico 5 / * kg -
Ritiro di stampaggio, parallelo 0.3 / * % ISO 294-4, 2577
Ritiro di stampaggio, perpendicolare 0.7 / * % ISO 294-4, 2577
Proprietà Meccanichesecco/condUnitáNorma del test
ISO Data
Modulo a trazione 4200 / 3600 MPa ISO 527
Carico unitario a trazione 90 / 81 MPa ISO 527
Deformazione a snervamento 4 / 4 % ISO 527
Deformazione nominale a rottura 5 / 4 % ISO 527
Resistenza all'urto Charpy, +23°C 64 / 49 kJ/m² ISO 179/1eU
Type of failure C / C - -
Resistenza all'urto Charpy, -30°C 80 / 55 kJ/m² ISO 179/1eU
Type of failure C / C - -
Resistenzia all'urto Charpy con intaglio, +23°C 12 / 9 kJ/m² ISO 179/1eA
Type of failure C / C - -
Resistenzia all'urto Charpy con intaglio, -30°C 11 / 7 kJ/m² ISO 179/1eA
Type of failure C / C - -
Proprietà Termichesecco/condUnitáNorma del test
ISO Data
Temperatura di fusione, 10°C/min 178 / * °C ISO 11357-1/-3
Temp.di inflessione sotto carico, 1.80 MPa 160 / * °C ISO 75-1/-2
Temp.di inflessione sotto carico, 0.45 MPa 175 / * °C ISO 75-1/-2
Temp.di rammollimento Vicat, B 170 / * °C ISO 306
Coeff.di dilatazione termica lin., parallelo 80 / * E-6/K ISO 11359-1/-2
Reaz. al fuoco spess.nom. 1.5mm HB / * class IEC 60695-11-10
Spessore provato 1.6 / * mm -
Yellow Card disponibile sì / * - -
Yellow Card disponibile sì / * - -
Proprietà Elettrichesecco/condUnitáNorma del test
ISO Data
Costante dielettrica relativa, 100Hz 4 / 5.2 - IEC 62631-2-1
Costante dielettrica relativa, 1MHz 3.4 / 3.3 - IEC 62631-2-1
Fattore di dissipazione, 100Hz 380 / - E-4 IEC 62631-2-1
Fattore di dissipazione, 1MHz 260 / 450 E-4 IEC 62631-2-1
Resistività volumica >1E13 / 1.8E12 Ohm*m IEC 62631-3-1
Rigidità dielettrica 50 / 47 kV/mm IEC 60243-1
Res. Alle correnti striscianti superficiali 600 / - - IEC 60112
Altre Proprietàsecco/condUnitáNorma del test
Assorbimento d'acqua 1.3 / * % Sim. alla ISO 62
Assorbimento d'umidità 0.6 / * % Sim. alla ISO 62
Massa volumica 1120 / - kg/m³ ISO 1183
Preparazione ProvetteValoreUnitáNorma del test
ISO Data
Stamp. ad Iniezione, temp. di fusione 260 °C ISO 294
Stamp. ad Iniezione, temperatura dello stampo 80 °C ISO 294
Stamp. ad Iniezione, velocità media d'iniezione 200 mm/s ISO 294
Stamp. ad Iniezione, pressione di chiusura 70 MPa ISO 294
Funzioni
Viscosità-Velocità di taglio , VESTAMID® L-GF15, PA12-GF15, Evonik
Sforzo di taglio-Velocità di taglio , VESTAMID® L-GF15, PA12-GF15, Evonik
Modulo dinamico a taglio-temperatura , VESTAMID® L-GF15 (Secco), PA12-GF15, Evonik
Sforzi-deformazione , VESTAMID® L-GF15 (Secco), PA12-GF15, Evonik
Modulo secante-deformazione , VESTAMID® L-GF15 (Secco), PA12-GF15, Evonik
Sforzi-deformazioni (isocrona) 23°C, VESTAMID® L-GF15 (cond.), PA12-GF15, Evonik
Modulo di scorrimento-tempo 23°C, VESTAMID® L-GF15 (cond.), PA12-GF15, Evonik
Curva di scorrimento 23°C, VESTAMID® L-GF15 (cond.), PA12-GF15, Evonik
Modulo a taglio-temperatura , VESTAMID® L-GF15 (Secco), PA12-GF15, Evonik
Caratteristiche
Processabilità e Forma di Forni
Stampaggio ad Iniezione
Forma fisica disponibile
Pellet, Colore naturale
Additivi
Lubrificanti
Caratteristiche speciali
Stabilizzato o stabile al calore
Applicazioni
Automotive
Disponibilità geografica
Nord America, Europa, Asia Oceano Pacifico, South and Central America, Near East/Africa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com