Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAMID® Terra HS1851 - PA610-GF20 - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAMID® Terra HS1851:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vestamid datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Testo del prodotto
Medium viscosity, glass fiber–reinforced, easily demoldable, heat-stabilized polyamide 610 compound for efficient injection molding

VESTAMID® Terra HS1851 is a glass fiber-reinforced, heat-stabilized, medium-viscosity PA 610 compound for injection molding application. The material contains about 20% glass fibers, an ageing protective agent and processing aid for a fast and even form filling.

The carbonamide groups (-CO-NH-) of the polyamides form hydrogen bridge bonds between the chains of the macromolecules, thereby substantially promoting crystallinity and increasing their strength, melting point, resistance to chemicals and even water absorption. This is characteristic of all semi-crystalline polyamides.

Because of its semi-crystalline morphology VESTAMID® Terra HS1851 provides a high impact strength, excellent chemical resistance (e.g. against greases, oils, alkalis and saline solutions), a low coefficient of friction and high abrasion resistance.
 

VESTAMID® Terra HS1851 is supplied as cylindrical granules, ready for processing, in moisture-proof bags.

 

VESTAMID® Terra is a group of new polyamides, the monomers for which are based entirely or partly on renewable raw materials.
 

VESTAMID® Terra HS is the polycondensation product of 1,6-hexamethylene diamine (H) and 1,10-decanedioic acid (sebacic acid—S). Because sebacic acid is derived from castor oil, VESTAMID® Terra HS is a material that is partly based on bio-based and renewable resources.
 

The use of colorants may affect property values. 

For information about processing of VESTAMID®, please follow the general commendations about “Processing of VESTAMID® compounds”. 

The values presented are typical or average values, they do not constitute a specification.

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM OR VISIT OUR PRODUCT AT  WWW.VESTAMID.TERRA.COM
Caratteristiche Fisichesecco/condUnitáNorma del test
ISO Data
Indice di fusione di volume, MVR 21 / * cm³/10min ISO 1133
Temperatura 250 / * °C -
Carico 5 / * kg -
Ritiro di stampaggio, parallelo 0.4 / * % ISO 294-4, 2577
Ritiro di stampaggio, perpendicolare 0.7 / * % ISO 294-4, 2577
Proprietà Meccanichesecco/condUnitáNorma del test
ISO Data
Modulo a trazione 6000 / - MPa ISO 527
Carico unitario a rottura 131 / - MPa ISO 527
Deformazione a rottura 3.8 / - % ISO 527
Resistenza all'urto Charpy, +23°C 86 / - kJ/m² ISO 179/1eU
Type of failure C / - - -
Resistenza all'urto Charpy, -30°C 78 / - kJ/m² ISO 179/1eU
Type of failure C / - - -
Resistenzia all'urto Charpy con intaglio, +23°C 11 / - kJ/m² ISO 179/1eA
Type of failure C / - - -
Resistenzia all'urto Charpy con intaglio, -30°C 8.9 / - kJ/m² ISO 179/1eA
Type of failure C / - - -
Proprietà Termichesecco/condUnitáNorma del test
ISO Data
Temperatura di fusione, 10°C/min 223 / * °C ISO 11357-1/-3
Temperatura di transizione vetrosa, 10°C/min 49 / * °C ISO 11357-1/-2
Temp.di inflessione sotto carico, 1.80 MPa 204 / * °C ISO 75-1/-2
Temp.di inflessione sotto carico, 0.45 MPa 222 / * °C ISO 75-1/-2
Temp.di rammollimento Vicat, B 219 / * °C ISO 306
Coeff.di dilatazione termica lin., parallelo 26 / * E-6/K ISO 11359-1/-2
Coeff.di dilatazione termica lin., perpend. 124 / * E-6/K ISO 11359-1/-2
Altre Proprietàsecco/condUnitáNorma del test
Assorbimento d'acqua 2.6 / * % Sim. alla ISO 62
Massa volumica 1220 / - kg/m³ ISO 1183
Preparazione ProvetteValoreUnitáNorma del test
ISO Data
Stamp. ad Iniezione, temp. di fusione 260 °C ISO 294
Stamp. ad Iniezione, temperatura dello stampo 80 °C ISO 294
Stamp. ad Iniezione, velocità media d'iniezione 200 mm/s ISO 294
Caratteristiche
Processabilità e Forma di Forni
Stampaggio ad Iniezione
Forma fisica disponibile
Pellet
Caratteristiche speciali
Alto urto o modificato all'urto, Stabilizzato o stabile al calore
Caratteristiche
Grado tribologico
Resistenza Chimica
Resistenza agli alcali, Resistenza chimica generale, Resistenza al grasso, Resistenza all’olio
Certifications
Contiene risorse rinnovabili
Disponibilità geografica
Nord America, Europa, Asia Oceano Pacifico, South and Central America, Near East/Africa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com