Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAMID® L1833 NC - PA12-GF23 - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAMID® L1833 NC:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, cooling time calculation, CAE Interfaces

Check here, which other Vestamid datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Testo del prodotto

Medium-viscosity, heat-stabilized, glass fiber–reinforced compound based on Nylon 12

VESTAMID® L1833 is a 23% glass fiber-re­inforced, easily demoldable and heat-stabilized polyamide 12 compound.

 

Due to its mold release properties, VESTAMID® L1833 is suitable for the efficient production of injection molded parts with short cycle times.

 

Further advantages of VESTAMID® L1833 are the characteristic properties of polyamide 12 as low water absorption, good dimensional stability and almost the same properties at changing ambient humidity.

VESTAMID® L1833 is supplied as cylindrical granules, ready for processing, in moisture-proof bags.

 

The use of colorants may change property values.

Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at temperatures not exceeding 30°C.

For information about processing of VESTAMID®, please follow the general commendations about “Processing of VESTAMID® compounds”. 

The values presented are typical or average values, they do not constitute a specification.

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM
OR VISIT OUR PRODUCT AT  WWW.VESTAMID.COM

Caratteristiche Fisichesecco/condUnitáNorma del test
ISO Data
Indice di fusione di volume, MVR 50 / * cm³/10min ISO 1133
Temperatura 275 / * °C -
Carico 5 / * kg -
Ritiro di stampaggio, parallelo 0.2 / * % ISO 294-4, 2577
Ritiro di stampaggio, perpendicolare 0.7 / * % ISO 294-4, 2577
Densità del fuso 1080 kg/m³ -
Conduttività termica del fuso 0.26 W/(m K) -
Capacità termica specifica del fuso 2640 J/(kg K) -
Temperatura di estrazione 180 °C -
Proprietà Meccanichesecco/condUnitáNorma del test
ISO Data
Modulo a trazione 5500 / 4800 MPa ISO 527
Carico unitario a trazione 107 / 95 MPa ISO 527
Deformazione a snervamento 4 / 5 % ISO 527
Deformazione nominale a rottura 6 / 6.5 % ISO 527
Modulo di scorrimento a trazione, 1h * / 5000 MPa ISO 899-1
Modulo di scorrimento a trazione, 1000h * / 3700 MPa ISO 899-1
Resistenza all'urto Charpy, +23°C 86 / 70 kJ/m² ISO 179/1eU
Type of failure C / - - -
Resistenza all'urto Charpy, -30°C 95 / 75 kJ/m² ISO 179/1eU
Type of failure C / - - -
Resistenzia all'urto Charpy con intaglio, +23°C 21 / 23 kJ/m² ISO 179/1eA
Type of failure C / - - -
Resistenzia all'urto Charpy con intaglio, -30°C 16 / 17 kJ/m² ISO 179/1eA
Type of failure C / - - -
Proprietà Termichesecco/condUnitáNorma del test
ISO Data
Temperatura di fusione, 10°C/min 178 / * °C ISO 11357-1/-3
Temperatura di transizione vetrosa, 10°C/min 40 / * °C ISO 11357-1/-2
Temp.di inflessione sotto carico, 1.80 MPa 160 / * °C ISO 75-1/-2
Temp.di inflessione sotto carico, 0.45 MPa 175 / * °C ISO 75-1/-2
Temp.di rammollimento Vicat, B 175 / * °C ISO 306
Coeff.di dilatazione termica lin., parallelo 70 / * E-6/K ISO 11359-1/-2
Coeff.di dilatazione termica lin., perpend. 80 / * E-6/K ISO 11359-1/-2
Reaz. al fuoco spess.nom. 1.5mm HB / * class IEC 60695-11-10
Spessore provato 1.6 / * mm -
Yellow Card disponibile sì / * - -
Yellow Card disponibile sì / * - -
Proprietà Elettrichesecco/condUnitáNorma del test
ISO Data
Costante dielettrica relativa, 100Hz 4.1 / 5 - IEC 62631-2-1
Costante dielettrica relativa, 1MHz 3.4 / 4 - IEC 62631-2-1
Fattore di dissipazione, 100Hz 370 / 700 E-4 IEC 62631-2-1
Fattore di dissipazione, 1MHz 260 / 450 E-4 IEC 62631-2-1
Resistività volumica >1E13 / 2E12 Ohm*m IEC 62631-3-1
Resistività superficiale * / >1E15 Ohm IEC 62631-3-2
Rigidità dielettrica 41 / 45 kV/mm IEC 60243-1
Res. Alle correnti striscianti superficiali 600 / 600 - IEC 60112
Altre Proprietàsecco/condUnitáNorma del test
Assorbimento d'acqua 1.2 / * % Sim. alla ISO 62
Assorbimento d'umidità 0.6 / * % Sim. alla ISO 62
Massa volumica 1170 / 1170 kg/m³ ISO 1183
Preparazione ProvetteValoreUnitáNorma del test
ISO Data
Stamp. ad Iniezione, temp. di fusione 240 °C ISO 294
Stamp. ad Iniezione, temperatura dello stampo 80 °C ISO 294
Stamp. ad Iniezione, velocità media d'iniezione 200 mm/s ISO 294
Stamp. ad Iniezione, pressione di chiusura 70 MPa ISO 294
Funzioni
Viscosità-Velocità di taglio , VESTAMID® L1833 NC, PA12-GF23, Evonik
Sforzo di taglio-Velocità di taglio , VESTAMID® L1833 NC, PA12-GF23, Evonik
Sforzi-deformazione , VESTAMID® L1833 NC (Secco), PA12-GF23, Evonik
Modulo secante-deformazione , VESTAMID® L1833 NC (Secco), PA12-GF23, Evonik
Sforzi-deformazioni (isocrona) 23°C, VESTAMID® L1833 NC (cond.), PA12-GF23, Evonik
Modulo di scorrimento-tempo 23°C, VESTAMID® L1833 NC (cond.), PA12-GF23, Evonik
Curva di scorrimento 23°C, VESTAMID® L1833 NC (cond.), PA12-GF23, Evonik
Sforzi-deformazioni (isocrona) 100°C, VESTAMID® L1833 NC (cond.), PA12-GF23, Evonik
Modulo di scorrimento-tempo 100°C, VESTAMID® L1833 NC (cond.), PA12-GF23, Evonik
Curva di scorrimento 100°C, VESTAMID® L1833 NC (cond.), PA12-GF23, Evonik
Volume specifico-temperatura (pvT) , VESTAMID® L1833 NC, PA12-GF23, Evonik
Modulo a taglio-temperatura , VESTAMID® L1833 NC (Secco), PA12-GF23, Evonik
Caratteristiche
Processabilità e Forma di Forni
Stampaggio ad Iniezione
Forma fisica disponibile
Pellet, Colore naturale
Additivi
Lubrificanti
Caratteristiche speciali
Stabilizzato o stabile al calore
Disponibilità geografica
Nord America, Europa, Asia Oceano Pacifico, South and Central America, Near East/Africa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com