Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAMID® Terra DS16 - PA1010 - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAMID® Terra DS16:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vestamid datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Testo del prodotto

Medium-viscosity polyamide 1010

VESTAMID® Terra DS16 NC is a medium-viscosity PA 1010 basic polymer. VESTAMID® Terra DS16 is semi-crystalline, which is the reason for its high mechanical resistance and chemical stability. It absorbs only little water. As a result its mechanical properties vary little when exposed to changing environmental humidity, and the material features a high dimensional stability.
 
VESTAMID® Terra DS16 can be used to manufacture films with good transparency.

The high melting point of VESTAMID Terra DS16 compounds results in a high heat deflection temperature that can be advantageous for some applications.
 
VESTAMID® Terra DS16 occupies a position between the high-performance long-chain polyamides such as PA 12 and PA 1212 and the standard polyamides PA 6 and PA 66, which have a shorter chain length.

VESTAMID® Terra DS16 NC is supplied as cylindrical granules, ready for processing, in moisture-proof bags.
 
VESTAMID® Terra is a group of new poly­amides, the monomers for which are based entirely or partly on renewable raw materials.

VESTAMID® Terra DS is the polycondensation product of 1,10-decamethylene diamine (D) and 1,10-dodecanedioic acid (sebacic acid-S). Because both monomers are extracted from castor oil, VESTAMID® Terra DS is based on natural, bio-based and renewable resources up to 100%.

The results shown have been generated from a low number of production lots. Therefore, they are preliminary and not yet the result of a statistical evaluation. Therefore they must not be used to establish specifications.

For information about processing of VESTAMID®, please follow the general commendations about “Processing of VESTAMID® compounds”. 

The values presented are typical or average values, they do not constitute a specification.

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM
OR VISIT OUR PRODUCT AT  WWW.VESTAMID.TERRA.COM

Caratteristiche Fisichesecco/condUnitáNorma del test
ISO Data
Ritiro di stampaggio, parallelo 1.4 / * % ISO 294-4, 2577
Ritiro di stampaggio, perpendicolare 1.5 / * % ISO 294-4, 2577
Proprietà Meccanichesecco/condUnitáNorma del test
ISO Data
Modulo a trazione 1700 / 1250 MPa ISO 527
Carico unitario a trazione 54 / 48 MPa ISO 527
Deformazione a snervamento 5 / 22 % ISO 527
Deformazione nominale a rottura >50 / >50 % ISO 527
Resistenza all'urto Charpy, +23°C N / N kJ/m² ISO 179/1eU
Resistenza all'urto Charpy, -30°C N / N kJ/m² ISO 179/1eU
Resistenzia all'urto Charpy con intaglio, +23°C 7 / 7 kJ/m² ISO 179/1eA
Type of failure C / C - -
Resistenzia all'urto Charpy con intaglio, -30°C 7 / 5 kJ/m² ISO 179/1eA
Type of failure C / C - -
Proprietà Termichesecco/condUnitáNorma del test
ISO Data
Temperatura di fusione, 10°C/min 200 / * °C ISO 11357-1/-3
Temperatura di transizione vetrosa, 10°C/min 37 / * °C ISO 11357-1/-2
Temp.di inflessione sotto carico, 1.80 MPa 55 / * °C ISO 75-1/-2
Temp.di inflessione sotto carico, 0.45 MPa 136 / * °C ISO 75-1/-2
Temp.di rammollimento Vicat, B 171 / * °C ISO 306
Coeff.di dilatazione termica lin., parallelo 115 / * E-6/K ISO 11359-1/-2
Coeff.di dilatazione termica lin., perpend. 135 / * E-6/K ISO 11359-1/-2
Reaz. al fuoco spess.nom. 1.5mm HB / * class IEC 60695-11-10
Spessore provato 1.6 / * mm -
Proprietà Elettrichesecco/condUnitáNorma del test
ISO Data
Costante dielettrica relativa, 100Hz 3.6 / - - IEC 62631-2-1
Costante dielettrica relativa, 1MHz 3.1 / - - IEC 62631-2-1
Resistività volumica >1E13 / 8.3E11 Ohm*m IEC 62631-3-1
Rigidità dielettrica 37 / - kV/mm IEC 60243-1
Altre Proprietàsecco/condUnitáNorma del test
Assorbimento d'acqua 1.8 / * % Sim. alla ISO 62
Assorbimento d'umidità 1.4 / * % Sim. alla ISO 62
Massa volumica 1040 / - kg/m³ ISO 1183
Caratteristiche
Processabilità e Forma di Forni
Stampaggio ad Iniezione, Estrusione Film, Altre Estrusioni
Forma fisica disponibile
Pellet, Granuli
Caratteristiche speciali
Stabilizzato o stabile al calore, Trasparente
Resistenza Chimica
Resistenza chimica generale
Certifications
Contiene risorse rinnovabili
Disponibilità geografica
Nord America, Europa, Asia Oceano Pacifico, South and Central America, Near East/Africa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com