Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTODUR® X4877 NC - PBT-I-GF30 - Evonik Operations GmbH

Material Data Center offers the following functions for VESTODUR® X4877 NC:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Vestodur datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Testo del prodotto

Easy-flow, glass fiber-reinforced polybutylene terephthalate compound with increased impact strength

VESTODUR® X4877 is an easy-flow, glass  fiber-reinforced (30%) polybutylene tereph­thalate compound (PBT) with increased impact strength for injection molding.

 

This compound is especially suitable for the manufacture of parts which are subjected to  high mechanical and thermal loads. Compared with commonly used glass fiber-reinforced

PBT compounds with a similar stiffness VESTODUR® X4877 has an increased impact strength and also a higher strain at break.

 

VESTODUR® X4877 is supplied as cylindrical pellets in polyethylene packaging.

 

For further information about processing of VESTODUR® X4877, please follow the general recommendations in our brochure "VESTODUR® Handling and Processing".

 

Pigmentation may affect values.
 

Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at temperatures not exceeding 30°C.


FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM 
OR VISIT OUR PRODUCT AT WWW.VESTODUR.COM

Caratteristiche Fisichesecco/condUnitáNorma del test
ISO Data
Indice di fusione di volume, MVR 20 / * cm³/10min ISO 1133
Temperatura 250 / * °C -
Carico 2.16 / * kg -
Ritiro di stampaggio, parallelo 0.3 / * % ISO 294-4, 2577
Ritiro di stampaggio, perpendicolare 1.0 / * % ISO 294-4, 2577
Proprietà Meccanichesecco/condUnitáNorma del test
ISO Data
Modulo a trazione 5200 / - MPa ISO 527
Carico unitario a rottura 100 / - MPa ISO 527
Deformazione a rottura 5.5 / - % ISO 527
Modulo di scorrimento a trazione, 1h * / 5200 MPa ISO 899-1
Modulo di scorrimento a trazione, 1000h * / 4500 MPa ISO 899-1
Resistenza all'urto Charpy, +23°C 80 / - kJ/m² ISO 179/1eU
Type of failure C / - - -
Resistenzia all'urto Charpy con intaglio, +23°C 16 / - kJ/m² ISO 179/1eA
Type of failure C / - - -
Resistenzia all'urto Charpy con intaglio, -30°C 13 / - kJ/m² ISO 179/1eA
Type of failure C / - - -
Durezza Shore D 79 / * - ISO 7619-1
Proprietà Termichesecco/condUnitáNorma del test
ISO Data
Temperatura di fusione, 10°C/min 200 / * °C ISO 11357-1/-3
Temp.di inflessione sotto carico, 1.80 MPa 175 / * °C ISO 75-1/-2
Temp.di inflessione sotto carico, 0.45 MPa 195 / * °C ISO 75-1/-2
Temp.di rammollimento Vicat, B 165 / * °C ISO 306
Coeff.di dilatazione termica lin., parallelo 50 / * E-6/K ISO 11359-1/-2
Reaz. al fuoco spess.nom. 1.5mm HB / * class IEC 60695-11-10
Spessore provato 1.6 / * mm -
Reazione al fuoco a spessore h HB / * class IEC 60695-11-10
Spessore provato 0.8 / * mm -
Proprietà Elettrichesecco/condUnitáNorma del test
ISO Data
Costante dielettrica relativa, 100Hz 4.7 / - - IEC 62631-2-1
Fattore di dissipazione, 100Hz 200 / - E-4 IEC 62631-2-1
Resistività volumica 1E12 / - Ohm*m IEC 62631-3-1
Resistività superficiale * / 1E13 Ohm IEC 62631-3-2
Res. Alle correnti striscianti superficiali 600 / - - IEC 60112
Altre Proprietàsecco/condUnitáNorma del test
Assorbimento d'acqua 0.25 / * % Sim. alla ISO 62
Massa volumica 1490 / - kg/m³ ISO 1183
Funzioni
Modulo dinamico a taglio-temperatura , VESTODUR® X4877 NC (Secco), PBT-I-GF30, Evonik
Volume specifico-temperatura (pvT) , VESTODUR® X4877 NC, PBT-I-GF30, Evonik
Caratteristiche
Processabilità e Forma di Forni
Stampaggio ad Iniezione
Forma fisica disponibile
Pellet, Colore naturale
Additivi
Lubrificanti, Agente di distacco
Caratteristiche speciali
Alto urto o modificato all'urto, Stabilizzato o stabile al calore
Disponibilità geografica
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.